MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Nilit FRIANYL B63 HS-GV15 Nylon 6 for injection molding, 15% glass fiber reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Glass Fiber Filled

Material Notes: Nylon 6 for injection molding, high impact modified.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ISO 1183
Water Absorption 2.0 - 3.0 %2.0 - 3.0 %ISO 62
Water Absorption at Saturation 7.0 - 8.0 %7.0 - 8.0 %ISO 62
Viscosity Measurement 145145Viscosity index; ISO 307
Linear Mold Shrinkage 0.010 - 0.018 cm/cm0.010 - 0.018 in/inFRISETTA Test Method
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 100 MPa14500 psiISO 2039-1
Tensile Strength at Break 105 MPa15200 psiISO 527
Elongation at Break 11 %11 %ISO 527
Tensile Modulus 4.50 GPa653 ksiISO 527
Flexural Strength 110 MPa16000 psiISO 178
Flexural Modulus 4.00 GPa580 ksiISO 178
Charpy Impact Unnotched 5.50 J/cm²26.2 ft-lb/in²DIN 53453
 NBNBISO 179/1eU
 6.00 J/cm²
@Temperature -40.0 °C
28.6 ft-lb/in²
@Temperature -40.0 °F
DIN 53453
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 1.50 J/cm²7.14 ft-lb/in²DIN 53453
 1.90 J/cm²9.04 ft-lb/in²ISO 179/1eA
 1.40 J/cm²
@Temperature -30.0 °C
6.66 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 93
Dissipation Factor 0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
IEC 250
Comparative Tracking Index 550 V550 VCTI 100; IEC 112
 
Thermal PropertiesMetricEnglishComments
Melting Point 221 °C430 °FISO 3146 DSC
Maximum Service Temperature, Air 100 °C212 °FContinuous; FRISETTA Test Method
Deflection Temperature at 0.46 MPa (66 psi) 200 °C392 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 160 °C320 °FISO 75

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Nilit FRIANYL B63 GV15 Nylon 6 for injection molding, 15% glass fiber reinforced
Celanese Nilit FRIANYL B63 V2 Nylon 6.6 for injection molding
Celanese Nilit FRIANYL B63 V0 Nylon 6.6 for injection molding
Celanese Nilit FRIANYL B63 HS-GV30 Nylon 6 for injection molding, 30% glass fiber reinforced

PFRI134 / 39055

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.