MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Hytrel® RS R4275 BK316 Polyester Elastomer TPC-ET
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polyester, TP; Polyester Thermoplastic Elastomer

Material Notes: 55 Shore D Renewably Sourced High Viscosity Polyester Elastomer with Good Heat Ageing Protection Developed for Blow Molding

Former DuPont product acquired by Celanese in 2022.

Key Words: TPC-ET
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.00 g/cc0.0361 lb/in³
 1.17 g/cc0.0423 lb/in³ISO 1183
Water Absorption 0.50 %
@Thickness 2.00 mm
0.50 %
@Thickness 0.0787 in
Sim. to ISO 62
Moisture Absorption 0.200 %
@Thickness 2.00 mm
0.200 %
@Thickness 0.0787 in
Sim. to ISO 62
Linear Mold Shrinkage, Transverse 0.019 cm/cm0.019 in/inISO 294-4 2577
Melt Flow  6.0 g/10 min
@Load 10.0 kg,
Temperature 230 °C
6.0 g/10 min
@Load 22.0 lb,
Temperature 446 °F
cm³/10min; ISO 1133
 6.0 g/10 min
@Load 10.0 kg,
Temperature 230 °C
6.0 g/10 min
@Load 22.0 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 505015s; ISO 868
Tensile Strength at Break 35.0 MPa5080 psiISO 527-1/-2
Elongation at Break >= 300 %>= 300 %ISO 527-1/-2
Tensile Modulus 0.150 GPa21.8 ksiISO 527-1/-2
 0.0467 GPa
@Temperature 110 °C
6.77 ksi
@Temperature 230 °F
Dynamic; ISO 11403-1 -2
 0.164 GPa
@Temperature 30.0 °C
23.7 ksi
@Temperature 86.0 °F
Dynamic; ISO 11403-1 -2
 0.456 GPa
@Temperature -20.0 °C
66.1 ksi
@Temperature -4.00 °F
Dynamic; ISO 11403-1 -2
 2.49 GPa
@Temperature -70.0 °C
361 ksi
@Temperature -94.0 °F
Dynamic; ISO 11403-1 -2
 3.15 GPa
@Temperature -100 °C
457 ksi
@Temperature -148 °F
Dynamic; ISO 11403-1 -2
Charpy Impact Unnotched NBNBISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched NBNBISO 179/1eA
 4.50 J/cm²
@Temperature -40.0 °C
21.4 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eA
 16.0 J/cm²
@Temperature -30.0 °C
76.1 ft-lb/in²
@Temperature -22.0 °F
Partial Break; ISO 179/1eA
Tensile Impact Strength 500 kJ/m²238 ft-lb/in²notched; ISO 8256/1
Tensile Creep Modulus, 1 hour  30.8 MPa
@Pressure 3.50 MPa,
Temperature 100 °C
4470 psi
@Pressure 508 psi,
Temperature 212 °F
ISO 11403-1 -2
 35.2 MPa
@Pressure 3.00 MPa,
Temperature 100 °C
5110 psi
@Pressure 435 psi,
Temperature 212 °F
ISO 11403-1 -2
 39.6 MPa
@Pressure 2.50 MPa,
Temperature 100 °C
5750 psi
@Pressure 363 psi,
Temperature 212 °F
ISO 11403-1 -2
 43.737 MPa
@Pressure 2.00 MPa,
Temperature 100 °C
6343.5 psi
@Pressure 290 psi,
Temperature 212 °F
ISO 11403-1 -2
 44.967 MPa
@Pressure 5.00 MPa,
Temperature 80.0 °C
6521.9 psi
@Pressure 725 psi,
Temperature 176 °F
ISO 11403-1 -2
 47.5 MPa
@Pressure 1.50 MPa,
Temperature 100 °C
6880 psi
@Pressure 218 psi,
Temperature 212 °F
ISO 11403-1 -2
 50.3 MPa
@Pressure 1.00 MPa,
Temperature 100 °C
7300 psi
@Pressure 145 psi,
Temperature 212 °F
ISO 11403-1 -2
 52.1 MPa
@Pressure 0.500 MPa,
Temperature 100 °C
7560 psi
@Pressure 72.5 psi,
Temperature 212 °F
ISO 11403-1 -2
 53.9 MPa
@Pressure 4.00 MPa,
Temperature 80.0 °C
7820 psi
@Pressure 580 psi,
Temperature 176 °F
ISO 11403-1 -2
 62.8 MPa
@Pressure 3.00 MPa,
Temperature 80.0 °C
9110 psi
@Pressure 435 psi,
Temperature 176 °F
ISO 11403-1 -2
 69.3 MPa
@Pressure 7.00 MPa,
Temperature 40.0 °C
10100 psi
@Pressure 1020 psi,
Temperature 104 °F
ISO 11403-1 -2
 70.4 MPa
@Pressure 2.00 MPa,
Temperature 80.0 °C
10200 psi
@Pressure 290 psi,
Temperature 176 °F
ISO 11403-1 -2
 75.6 MPa
@Pressure 1.00 MPa,
Temperature 80.0 °C
11000 psi
@Pressure 145 psi,
Temperature 176 °F
ISO 11403-1 -2
 78.2 MPa
@Pressure 6.00 MPa,
Temperature 40.0 °C
11300 psi
@Pressure 870 psi,
Temperature 104 °F
ISO 11403-1 -2
 87.1 MPa
@Pressure 5.00 MPa,
Temperature 40.0 °C
12600 psi
@Pressure 725 psi,
Temperature 104 °F
ISO 11403-1 -2
 88.0 MPa
@Pressure 8.00 MPa,
Temperature 23.0 °C
12800 psi
@Pressure 1160 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 95.5 MPa
@Pressure 4.00 MPa,
Temperature 40.0 °C
13900 psi
@Pressure 580 psi,
Temperature 104 °F
ISO 11403-1 -2
 103 MPa
@Pressure 3.00 MPa,
Temperature 40.0 °C
14900 psi
@Pressure 435 psi,
Temperature 104 °F
ISO 11403-1 -2
 106 MPa
@Pressure 6.00 MPa,
Temperature 23.0 °C
15400 psi
@Pressure 870 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 108 MPa
@Pressure 2.00 MPa,
Temperature 40.0 °C
15700 psi
@Pressure 290 psi,
Temperature 104 °F
ISO 11403-1 -2
 112 MPa
@Pressure 1.00 MPa,
Temperature 40.0 °C
16200 psi
@Pressure 145 psi,
Temperature 104 °F
ISO 11403-1 -2
 122 MPa
@Pressure 4.00 MPa,
Temperature 23.0 °C
17700 psi
@Pressure 580 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 133 MPa
@Pressure 2.00 MPa,
Temperature 23.0 °C
19300 psi
@Pressure 290 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 140 MPa
@Time 3600 sec
20300 psi
@Time 1.00 hour
ISO 899-1
Tensile Creep Modulus, 1000 hours  21.7 MPa
@Pressure 3.50 MPa,
Temperature 100 °C
3150 psi
@Pressure 508 psi,
Temperature 212 °F
ISO 11403-1 -2
 25.2 MPa
@Pressure 3.00 MPa,
Temperature 100 °C
3660 psi
@Pressure 435 psi,
Temperature 212 °F
ISO 11403-1 -2
 28.6 MPa
@Pressure 2.50 MPa,
Temperature 100 °C
4150 psi
@Pressure 363 psi,
Temperature 212 °F
ISO 11403-1 -2
 31.9 MPa
@Pressure 2.00 MPa,
Temperature 100 °C
4630 psi
@Pressure 290 psi,
Temperature 212 °F
ISO 11403-1 -2
 33.9 MPa
@Pressure 5.00 MPa,
Temperature 80.0 °C
4920 psi
@Pressure 725 psi,
Temperature 176 °F
ISO 11403-1 -2
 34.8 MPa
@Pressure 1.50 MPa,
Temperature 100 °C
5050 psi
@Pressure 218 psi,
Temperature 212 °F
ISO 11403-1 -2
 37.2 MPa
@Pressure 1.00 MPa,
Temperature 100 °C
5400 psi
@Pressure 145 psi,
Temperature 212 °F
ISO 11403-1 -2
 38.7 MPa
@Pressure 0.500 MPa,
Temperature 100 °C
5610 psi
@Pressure 72.5 psi,
Temperature 212 °F
ISO 11403-1 -2
 41.1 MPa
@Pressure 4.00 MPa,
Temperature 80.0 °C
5960 psi
@Pressure 580 psi,
Temperature 176 °F
ISO 11403-1 -2
 48.3 MPa
@Pressure 3.00 MPa,
Temperature 80.0 °C
7000 psi
@Pressure 435 psi,
Temperature 176 °F
ISO 11403-1 -2
 49.7 MPa
@Pressure 7.00 MPa,
Temperature 40.0 °C
7210 psi
@Pressure 1020 psi,
Temperature 104 °F
ISO 11403-1 -2
 54.6 MPa
@Pressure 2.00 MPa,
Temperature 80.0 °C
7910 psi
@Pressure 290 psi,
Temperature 176 °F
ISO 11403-1 -2
 56.6 MPa
@Pressure 6.00 MPa,
Temperature 40.0 °C
8220 psi
@Pressure 870 psi,
Temperature 104 °F
ISO 11403-1 -2
 57.9 MPa
@Pressure 8.00 MPa,
Temperature 23.0 °C
8400 psi
@Pressure 1160 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 59.0 MPa
@Pressure 1.00 MPa,
Temperature 80.0 °C
8560 psi
@Pressure 145 psi,
Temperature 176 °F
ISO 11403-1 -2
 63.8 MPa
@Pressure 5.00 MPa,
Temperature 40.0 °C
9250 psi
@Pressure 725 psi,
Temperature 104 °F
ISO 11403-1 -2
 70.2 MPa
@Pressure 6.00 MPa,
Temperature 23.0 °C
10200 psi
@Pressure 870 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 70.2 MPa
@Pressure 4.00 MPa,
Temperature 40.0 °C
10200 psi
@Pressure 580 psi,
Temperature 104 °F
ISO 11403-1 -2
 75.9 MPa
@Pressure 3.00 MPa,
Temperature 40.0 °C
11000 psi
@Pressure 435 psi,
Temperature 104 °F
ISO 11403-1 -2
 80.3 MPa
@Pressure 2.00 MPa,
Temperature 40.0 °C
11700 psi
@Pressure 290 psi,
Temperature 104 °F
ISO 11403-1 -2
 81.1 MPa
@Pressure 4.00 MPa,
Temperature 23.0 °C
11800 psi
@Pressure 580 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 83.3 MPa
@Pressure 1.00 MPa,
Temperature 40.0 °C
12100 psi
@Pressure 145 psi,
Temperature 104 °F
ISO 11403-1 -2
 88.9 MPa
@Pressure 2.00 MPa,
Temperature 23.0 °C
12900 psi
@Pressure 290 psi,
Temperature 73.4 °F
ISO 11403-1 -2
 90.0 MPa
@Time 3.60e+6 sec
13100 psi
@Time 1000 hour
ISO 899-1
Tear Strength 140 kN/m799 pliparallel; ISO 34-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 180 µm/m-°C100 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 190 µm/m-°C106 µin/in-°FISO 11359-1/-2
Specific Heat Capacity 2.10 J/g-°C0.502 BTU/lb-°F
Thermal Conductivity 0.150 W/m-K1.04 BTU-in/hr-ft²-°Fof melt
Melting Point 190 °C374 °F10°C/min; ISO 11357-1/-3
Brittleness Temperature -70.0 °C-94.0 °FISO 974
Glass Transition Temp, Tg -30.0 °C-22.0 °F10°C/min; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
 
Descriptive Properties
Delivery formPellets
Eff. thermal diffusivity5.44E-08 m²/s
Part Marking Code>TPC-ET<ISO 11469
ProcessingBlow Molding
 Calandering
 Casting
 Coatable
 Film Extrusion
 Other Extrusion
 Profile Extrusion
 Sheet Extrusion
 Thermoforming
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationTPC-ETISO 1043
Special characteristicsHeat stabilized or stable to heat

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Riteflex® 663 TPC, Unfilled
Celanese Riteflex® 672 TPC, Unfilled
Celanese Hytrel® HTR8341C BK320 TPC-ET
Celanese Hytrel® RS R4275 BK316 Polyester Elastomer TPC-ET (with Extended Stress-Strain Tabular Data)
Celanese Riteflex® 640A TPC, Unfilled

PZDSY5236 / 161063

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.