MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

INEOS Styrolution Polystyrol 165 H GR 2 PS
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Molded, Unreinforced

Material Notes: Description: Polystyrol 165 H is a high molecular weight, good flowing grade, often blended with high impact extrusion grades.

Applications: In blends with high impact Polystyrene or Styrolux; thermoformed articles for high impact resistant packagings of dairy products, breakers for cold beverages. As material for physically or chemically foamed sheet, eg. for meat trays or labels.

Information provided by STYROLUTION, which is a joint venture between BASF and INEOS

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.045 g/cc0.03775 lb/in³ISO 1183
Water Absorption <= 0.10 %<= 0.10 %ISO 62
Moisture Absorption at Equilibrium <= 0.10 %<= 0.10 %23°C/50% RH; ISO 62
Melt Flow 3.553 g/10 min
@Load 5.00 kg,
Temperature 200 °C
3.553 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 150 MPa
@Load 36.5 kg,
Time 30.0 sec
21800 psi
@Load 80.5 lb,
Time 0.00833 hour
ISO 2039-1
Tensile Strength at Break 52.0 MPa7540 psiISO 527-1/-2
Elongation at Break 2.0 %2.0 %ISO 527-1/-2
Tensile Modulus 3.30 GPa479 ksiISO 527-1/-2
Flexural Strength 86.0 MPa12500 psiISO 178
Shear Modulus 1.40 GPa203 ksiISO 6721-2
Charpy Impact Unnotched <= 2.50 J/cm²<= 11.9 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 0.300 J/cm²1.43 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmIEC 60093
Surface Resistance >= 1.00e+14 ohm>= 1.00e+14 ohmIEC 60093
Dielectric Constant  2.5
@Frequency 1e+6 Hz
2.5
@Frequency 1e+6 Hz
IEC 60250
 2.5
@Frequency 100 Hz
2.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 135 kV/mm3430 kV/inK20/P50; IEC 60243-1
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 84.0 °C183 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 76.0 °C169 °FISO 75-1/-2
Vicat Softening Point 89.0 °C192 °FVST/B/50; ISO 306
 97.0 °C207 °FVST/A/120; ISO 306
Flammability, UL94  HB
@Diameter 1.60 mm
HB
@Diameter 0.0630 in
IEC 60695-11-10
 HB
@Diameter 3.18 mm
HB
@Diameter 0.125 in
IEC 60695-11-10
 
Processing PropertiesMetricEnglishComments
Melt Temperature 200 - 240 °C392 - 464 °FFlat film
 180 - 280 °C356 - 536 °FInjection Molding
Mold Temperature 10.0 - 60.0 °C50.0 - 140 °FInjection Molding
 
Descriptive Properties
ColorCrystal Clear 00013
Commercial StatusEurope
Primary Processing TechniqueInjection Molding and Extrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman Diamond TR 5000
Total PSC 500 Polystyrene
BASF Polystyrol® 165 H Polystyrene (Europe)
Chevron Phillips EA3025 Crystal Polystyrene
INEOS Styrolution PS 116 N/L GPPS

PBASG0625 / 132258

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.