Physical Properties | Metric | English | Comments |
---|
Density | 8.44 g/cc | 0.305 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength, Ultimate | 985 MPa | 143000 psi |
Tensile Strength, Yield | 660 MPa @Strain 0.2 % | 95700 psi @Strain 0.2 % |
Elongation at Break | 17 % | 17 % |
Modulus of Elasticity | 208 GPa | 30200 ksi |
| 126 GPa @Temperature 1000 °C | 18300 ksi @Temperature 1830 °F |
| 142 GPa @Temperature 900 °C | 20600 ksi @Temperature 1650 °F |
| 153 GPa @Temperature 800 °C | 22200 ksi @Temperature 1470 °F |
| 163 GPa @Temperature 700 °C | 23600 ksi @Temperature 1290 °F |
| 171 GPa @Temperature 600 °C | 24800 ksi @Temperature 1110 °F |
| 179 GPa @Temperature 500 °C | 26000 ksi @Temperature 932 °F |
| 186 GPa @Temperature 400 °C | 27000 ksi @Temperature 752 °F |
| 192 GPa @Temperature 300 °C | 27800 ksi @Temperature 572 °F |
| 199 GPa @Temperature 200 °C | 28900 ksi @Temperature 392 °F |
| 201 GPa @Temperature 100 °C | 29200 ksi @Temperature 212 °F |
Charpy Impact | 7.00 J | 5.16 ft-lb |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.000129 ohm-cm | 0.000129 ohm-cm |
| 0.000132 ohm-cm @Temperature 100 °C | 0.000132 ohm-cm @Temperature 212 °F |
| 0.000134 ohm-cm @Temperature 200 °C | 0.000134 ohm-cm @Temperature 392 °F |
| 0.000135 ohm-cm @Temperature 300 °C | 0.000135 ohm-cm @Temperature 572 °F |
| 0.000135 ohm-cm @Temperature 1000 °C | 0.000135 ohm-cm @Temperature 1830 °F |
| 0.000136 ohm-cm @Temperature 900 °C | 0.000136 ohm-cm @Temperature 1650 °F |
| 0.000136 ohm-cm @Temperature 400 °C | 0.000136 ohm-cm @Temperature 752 °F |
| 0.000137 ohm-cm @Temperature 500 °C | 0.000137 ohm-cm @Temperature 932 °F |
| 0.000137 ohm-cm @Temperature 800 °C | 0.000137 ohm-cm @Temperature 1470 °F |
| 0.000138 ohm-cm @Temperature 600 °C | 0.000138 ohm-cm @Temperature 1110 °F |
| 0.000138 ohm-cm @Temperature 700 °C | 0.000138 ohm-cm @Temperature 1290 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.8 µm/m-°C @Temperature 25.0 - 100 °C | 7.11 µin/in-°F @Temperature 77.0 - 212 °F |
| 13.1 µm/m-°C @Temperature 25.0 - 200 °C | 7.28 µin/in-°F @Temperature 77.0 - 392 °F |
| 13.4 µm/m-°C @Temperature 25.0 - 300 °C | 7.44 µin/in-°F @Temperature 77.0 - 572 °F |
| 13.8 µm/m-°C @Temperature 25.0 - 400 °C | 7.67 µin/in-°F @Temperature 77.0 - 752 °F |
| 14.2 µm/m-°C @Temperature 25.0 - 500 °C | 7.89 µin/in-°F @Temperature 77.0 - 932 °F |
| 14.8 µm/m-°C @Temperature 25.0 - 600 °C | 8.22 µin/in-°F @Temperature 77.0 - 1110 °F |
| 15.4 µm/m-°C @Temperature 25.0 - 700 °C | 8.56 µin/in-°F @Temperature 77.0 - 1290 °F |
| 16.0 µm/m-°C @Temperature 25.0 - 800 °C | 8.89 µin/in-°F @Temperature 77.0 - 1470 °F |
| 16.7 µm/m-°C @Temperature 25.0 - 900 °C | 9.28 µin/in-°F @Temperature 77.0 - 1650 °F |
| 17.4 µm/m-°C @Temperature 25.0 - 1000 °C | 9.67 µin/in-°F @Temperature 77.0 - 1830 °F |
Specific Heat Capacity | 0.410 J/g-°C | 0.0980 BTU/lb-°F |
| 0.428 J/g-°C @Temperature 100 °C | 0.102 BTU/lb-°F @Temperature 212 °F |
| 0.455 J/g-°C @Temperature 200 °C | 0.109 BTU/lb-°F @Temperature 392 °F |
| 0.477 J/g-°C @Temperature 300 °C | 0.114 BTU/lb-°F @Temperature 572 °F |
| 0.503 J/g-°C @Temperature 400 °C | 0.120 BTU/lb-°F @Temperature 752 °F |
| 0.527 J/g-°C @Temperature 500 °C | 0.126 BTU/lb-°F @Temperature 932 °F |
| 0.552 J/g-°C @Temperature 600 °C | 0.132 BTU/lb-°F @Temperature 1110 °F |
| 0.576 J/g-°C @Temperature 700 °C | 0.138 BTU/lb-°F @Temperature 1290 °F |
| 0.600 J/g-°C @Temperature 800 °C | 0.143 BTU/lb-°F @Temperature 1470 °F |
| 0.625 J/g-°C @Temperature 900 °C | 0.149 BTU/lb-°F @Temperature 1650 °F |
| 0.648 J/g-°C @Temperature 1000 °C | 0.155 BTU/lb-°F @Temperature 1830 °F |
Thermal Conductivity | 9.80 W/m-K | 68.0 BTU-in/hr-ft²-°F |
| 10.9 W/m-K @Temperature 100 °C | 75.6 BTU-in/hr-ft²-°F @Temperature 212 °F |
| 12.5 W/m-K @Temperature 200 °C | 86.8 BTU-in/hr-ft²-°F @Temperature 392 °F |
| 13.9 W/m-K @Temperature 300 °C | 96.5 BTU-in/hr-ft²-°F @Temperature 572 °F |
| 15.3 W/m-K @Temperature 400 °C | 106 BTU-in/hr-ft²-°F @Temperature 752 °F |
| 16.9 W/m-K @Temperature 500 °C | 117 BTU-in/hr-ft²-°F @Temperature 932 °F |
| 18.3 W/m-K @Temperature 600 °C | 127 BTU-in/hr-ft²-°F @Temperature 1110 °F |
| 19.8 W/m-K @Temperature 700 °C | 137 BTU-in/hr-ft²-°F @Temperature 1290 °F |
| 21.5 W/m-K @Temperature 800 °C | 149 BTU-in/hr-ft²-°F @Temperature 1470 °F |
| 23.4 W/m-K @Temperature 900 °C | 162 BTU-in/hr-ft²-°F @Temperature 1650 °F |
| 25.6 W/m-K @Temperature 1000 °C | 178 BTU-in/hr-ft²-°F @Temperature 1830 °F |
Melting Point | 1290 - 1350 °C | 2350 - 2460 °F |
Solidus | 1290 °C | 2350 °F |
Liquidus | 1350 °C | 2460 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | <= 0.40 % | <= 0.40 % |
Carbon, C | <= 0.10 % | <= 0.10 % |
Chromium, Cr | 21 % | 21 % |
Cobalt, Co | <= 1.0 % | <= 1.0 % |
Iron, Fe | <= 5.0 % | <= 5.0 % |
Manganese, Mn | <= 0.50 % | <= 0.50 % |
Molybdenum, Mo | 9.0 % | 9.0 % |
Nickel, Ni | 62 % | 62 % |
Niobium, Nb (Columbium, Cb) | 3.7 % | 3.7 % |
Silicon, Si | <= 0.50 % | <= 0.50 % |