MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

LyondellBasell Pro-fax 7823 Polypropylene Impact Copolymer, Fractional Melt Flow
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes:
Key Features: high extrudate melt strength, good cold impact resistance, good stiffness and impact balance, FDA acceptable

Applications: pipe, tubing, sheet, profiles, netting, blown containers and industrial components

Meets FDA requirements in 21 CFR 177.1520 for all food contact, including cooking applications.

Description: Pro-fax 7823 fractional melt flow polypropylene copolymer resin is designed for extrusion applications requiring high melt strength and excellent toughness. This resin is available in pellet form. It has passed USP Class VI testing, and has a UL yellow card RTI, which applies to all colors. This resin meets FDA requirements in the Code of Federal Regulations in 21 CFR 177.520 for all food contact, including cooking applications. All ingredients meet the chemical registration requirements of TSCA and DSL.

Information provided by Montell Polyolefins.

LyondellBasell is the successor company to Montell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ASTM D792B
Melt Flow 0.45 g/10 min
@Load 2.16 kg,
Temperature 230 °C
0.45 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 27.0 MPa3920 psiASTM D638
Elongation at Yield 11 %11 %ASTM D638
Flexural Modulus, 1% Secant 1100 MPa160000 psi0.05 in/min; ASTM D790A
Izod Impact, Notched NBNBASTM D256A
Impact Test 29.0 J
@Temperature -29.0 °C
21.4 ft-lb
@Temperature -20.2 °F
Montell drop weight impact strength
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °C190 °FASTM D648
UL RTI, Mechanical with Impact 115 °C
@Thickness >=1.02 mm
239 °F
@Thickness >=0.0400 in
Flammability, UL94 HB
@Thickness >=1.02 mm
HB
@Thickness >=0.0400 in
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.
USP Class VI YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Pro-fax 8523 Polypropylene Impact Copolymer
LyondellBasell Pro-fax 7624 Polypropylene Impact Copolymer, Heat- and Extraction-Resistant
LyondellBasell Pro-fax SV152 Polypropylene Impact Copolymer
LyondellBasell Montell SE191 Polypropylene Impact Copolymer
LyondellBasell Pro-fax 7531 Polypropylene Impact Copolymer

PMO189 / 53552

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.