Physical Properties | Metric | English | Comments |
---|
Density | 2.80 g/cc | 0.101 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 145 | 145 |
Hardness, Knoop | 184 | 184 |
Hardness, Rockwell A | 52.6 | 52.6 |
Hardness, Rockwell B | 86 | 86 |
Hardness, Vickers | 169 | 169 |
Tensile Strength, Ultimate | 550 MPa | 79800 psi |
| 552 MPa @Thickness 75.0 mm, Temperature 24.0 °C | 80100 psi @Thickness 2.95 in, Temperature 75.2 °F |
| 600 MPa @Thickness 75.0 mm, Temperature -28.0 °C | 87000 psi @Thickness 2.95 in, Temperature -18.4 °F |
| 621 MPa @Thickness 75.0 mm, Temperature -80.0 °C | 90100 psi @Thickness 2.95 in, Temperature -112 °F |
| 731 MPa @Thickness 75.0 mm, Temperature -196 °C | 106000 psi @Thickness 2.95 in, Temperature -321 °F |
| 876 MPa @Thickness 75.0 mm, Temperature -253 °C | 127000 psi @Thickness 2.95 in, Temperature -423 °F |
| 90.0 MPa @Thickness 75.0 mm, Temperature 232 °C, Time 3.60e+7 sec | 13100 psi @Thickness 2.95 in, Temperature 450 °F, Time 10000 hour |
| 97.0 MPa @Thickness 75.0 mm, Temperature 232 °C, Time 3.60e+6 sec | 14100 psi @Thickness 2.95 in, Temperature 450 °F, Time 1000 hour |
| 117 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 232 °C | 17000 psi @Thickness 2.95 in, Time 100 hour, Temperature 450 °F |
| 124 MPa @Thickness 75.0 mm, Temperature 204 °C, Time 3.60e+6 sec | 18000 psi @Thickness 2.95 in, Temperature 399 °F, Time 1000 hour |
| 124 MPa @Thickness 75.0 mm, Temperature 204 °C, Time 3.60e+7 sec | 18000 psi @Thickness 2.95 in, Temperature 399 °F, Time 10000 hour |
| 159 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 232 °C | 23100 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 450 °F |
| 165 MPa @Thickness 75.0 mm, Temperature 176 °C, Time 3.60e+7 sec | 23900 psi @Thickness 2.95 in, Temperature 349 °F, Time 10000 hour |
| 165 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 204 °C | 23900 psi @Thickness 2.95 in, Time 100 hour, Temperature 399 °F |
| 200 MPa @Thickness 75.0 mm, Temperature 176 °C, Time 3.60e+6 sec | 29000 psi @Thickness 2.95 in, Temperature 349 °F, Time 1000 hour |
| 228 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 204 °C | 33100 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 399 °F |
| 228 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 232 °C | 33100 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 450 °F |
| 241 MPa @Thickness 75.0 mm, Temperature 149 °C, Time 3.60e+7 sec | 35000 psi @Thickness 2.95 in, Temperature 300 °F, Time 10000 hour |
| 262 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 176 °C | 38000 psi @Thickness 2.95 in, Time 100 hour, Temperature 349 °F |
| 262 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 232 °C | 38000 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 450 °F |
| 310 MPa @Thickness 75.0 mm, Temperature 149 °C, Time 3.60e+6 sec | 45000 psi @Thickness 2.95 in, Temperature 300 °F, Time 1000 hour |
| 310 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 204 °C | 45000 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 399 °F |
| 324 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 204 °C | 47000 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 399 °F |
| 338 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 176 °C | 49000 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 349 °F |
| 365 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 176 °C | 52900 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 349 °F |
| 379 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 176 °C | 55000 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 349 °F |
| 393 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 149 °C | 57000 psi @Thickness 2.95 in, Time 100 hour, Temperature 300 °F |
| 427 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 149 °C | 61900 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 300 °F |
| 427 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 149 °C | 61900 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 300 °F |
| 427 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 149 °C | 61900 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 300 °F |
| 490 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 100 °C | 71100 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 212 °F |
| 490 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 100 °C | 71100 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 212 °F |
| 496 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 100 °C | 71900 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 212 °F |
| 496 MPa @Thickness 75.0 mm, Temperature 100 °C, Time 3.60e+7 sec | 71900 psi @Thickness 2.95 in, Temperature 212 °F, Time 10000 hour |
| 503 MPa @Thickness 75.0 mm, Temperature 100 °C, Time 360000 sec | 73000 psi @Thickness 2.95 in, Temperature 212 °F, Time 100 hour |
| 503 MPa @Thickness 75.0 mm, Temperature 100 °C, Time 3.60e+6 sec | 73000 psi @Thickness 2.95 in, Temperature 212 °F, Time 1000 hour |
| 552 MPa @Treatment Temp. 24.0 °C, Thickness 75.0 mm | 80100 psi @Treatment Temp. 75.2 °F, Thickness 2.95 in |
| 221 MPa @Time 3.60e+7 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 32100 psi @Time 10000 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 234 MPa @Time 3.60e+7 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 33900 psi @Time 10000 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 234 MPa @Time 3.60e+6 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 33900 psi @Time 1000 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 255 MPa @Time 3.60e+6 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 37000 psi @Time 1000 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 262 MPa @Time 3.60e+7 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 38000 psi @Time 10000 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 269 MPa @Time 360000 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 39000 psi @Time 100 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 317 MPa @Time 360000 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 46000 psi @Time 100 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 331 MPa @Time 3.60e+6 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 48000 psi @Time 1000 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 338 MPa @Time 36000 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 49000 psi @Time 10.0 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 352 MPa @Time 3.60e+7 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 51100 psi @Time 10000 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 393 MPa @Time 36000 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 57000 psi @Time 10.0 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 421 MPa @Time 360000 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 61100 psi @Time 100 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 441 MPa @Time 3.60e+6 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 64000 psi @Time 1000 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 448 MPa @Time 1800 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 65000 psi @Time 0.500 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 496 MPa @Time 36000 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 71900 psi @Time 10.0 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 503 MPa @Time 1800 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 73000 psi @Time 0.500 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 510 MPa @Time 360 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 74000 psi @Time 0.100 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 524 MPa @Time 360000 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 76000 psi @Time 100 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 524 MPa @Time 360 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 76000 psi @Time 0.100 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 538 MPa @Time 360 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 78000 psi @Time 0.100 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 538 MPa @Time 1800 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 78000 psi @Time 0.500 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 552 MPa @Time 360 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 80100 psi @Time 0.100 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 552 MPa @Time 1800 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 80100 psi @Time 0.500 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 552 MPa @Time 36000 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 80100 psi @Time 10.0 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 552 MPa @Time 360 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 80100 psi @Time 0.100 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 552 MPa @Time 1800 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 80100 psi @Time 0.500 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 552 MPa @Time 36000 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 80100 psi @Time 10.0 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 558 MPa @Time 360000 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 80900 psi @Time 100 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 558 MPa @Time 3.60e+7 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 80900 psi @Time 10000 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 565 MPa @Time 3.60e+6 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 81900 psi @Time 1000 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
Tensile Strength, Yield | 485 MPa | 70300 psi |
| 503 MPa @Thickness 75.0 mm, Temperature 24.0 °C | 73000 psi @Thickness 2.95 in, Temperature 75.2 °F |
| 552 MPa @Thickness 75.0 mm, Temperature -28.0 °C | 80100 psi @Thickness 2.95 in, Temperature -18.4 °F |
| 572 MPa @Thickness 75.0 mm, Temperature -80.0 °C | 83000 psi @Thickness 2.95 in, Temperature -112 °F |
| 676 MPa @Thickness 75.0 mm, Temperature -196 °C | 98000 psi @Thickness 2.95 in, Temperature -321 °F |
| 745 MPa @Thickness 75.0 mm, Temperature -253 °C | 108000 psi @Thickness 2.95 in, Temperature -423 °F |
| 76.0 MPa @Thickness 75.0 mm, Temperature 232 °C, Time 3.60e+7 sec | 11000 psi @Thickness 2.95 in, Temperature 450 °F, Time 10000 hour |
| 83.0 MPa @Thickness 75.0 mm, Temperature 232 °C, Time 3.60e+6 sec | 12000 psi @Thickness 2.95 in, Temperature 450 °F, Time 1000 hour |
| 90.0 MPa @Thickness 75.0 mm, Temperature 204 °C, Time 3.60e+7 sec | 13100 psi @Thickness 2.95 in, Temperature 399 °F, Time 10000 hour |
| 103 MPa @Thickness 75.0 mm, Temperature 204 °C, Time 3.60e+6 sec | 14900 psi @Thickness 2.95 in, Temperature 399 °F, Time 1000 hour |
| 103 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 232 °C | 14900 psi @Thickness 2.95 in, Time 100 hour, Temperature 450 °F |
| 131 MPa @Thickness 75.0 mm, Temperature 176 °C, Time 3.60e+7 sec | 19000 psi @Thickness 2.95 in, Temperature 349 °F, Time 10000 hour |
| 145 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 232 °C | 21000 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 450 °F |
| 179 MPa @Thickness 75.0 mm, Temperature 176 °C, Time 3.60e+6 sec | 26000 psi @Thickness 2.95 in, Temperature 349 °F, Time 1000 hour |
| 214 MPa @Thickness 75.0 mm, Temperature 149 °C, Time 3.60e+7 sec | 31000 psi @Thickness 2.95 in, Temperature 300 °F, Time 10000 hour |
| 214 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 204 °C | 31000 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 399 °F |
| 214 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 232 °C | 31000 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 450 °F |
| 221 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 204 °C | 32100 psi @Thickness 2.95 in, Time 100 hour, Temperature 399 °F |
| 241 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 176 °C | 35000 psi @Thickness 2.95 in, Time 100 hour, Temperature 349 °F |
| 241 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 232 °C | 35000 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 450 °F |
| 283 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 204 °C | 41000 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 399 °F |
| 296 MPa @Thickness 75.0 mm, Temperature 149 °C, Time 3.60e+6 sec | 42900 psi @Thickness 2.95 in, Temperature 300 °F, Time 1000 hour |
| 303 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 204 °C | 43900 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 399 °F |
| 324 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 176 °C | 47000 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 349 °F |
| 345 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 176 °C | 50000 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 349 °F |
| 345 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 176 °C | 50000 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 349 °F |
| 372 MPa @Thickness 75.0 mm, Time 360000 sec, Temperature 149 °C | 54000 psi @Thickness 2.95 in, Time 100 hour, Temperature 300 °F |
| 414 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 149 °C | 60000 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 300 °F |
| 414 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 149 °C | 60000 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 300 °F |
| 414 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 149 °C | 60000 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 300 °F |
| 462 MPa @Time 1800 sec, Thickness 75.0 mm, Temperature 100 °C | 67000 psi @Time 0.500 hour, Thickness 2.95 in, Temperature 212 °F |
| 476 MPa @Time 360 sec, Thickness 75.0 mm, Temperature 100 °C | 69000 psi @Time 0.100 hour, Thickness 2.95 in, Temperature 212 °F |
| 476 MPa @Time 36000 sec, Thickness 75.0 mm, Temperature 100 °C | 69000 psi @Time 10.0 hour, Thickness 2.95 in, Temperature 212 °F |
| 476 MPa @Thickness 75.0 mm, Temperature 100 °C, Time 3.60e+7 sec | 69000 psi @Thickness 2.95 in, Temperature 212 °F, Time 10000 hour |
| 483 MPa @Thickness 75.0 mm, Temperature 100 °C, Time 360000 sec | 70100 psi @Thickness 2.95 in, Temperature 212 °F, Time 100 hour |
| 483 MPa @Thickness 75.0 mm, Temperature 100 °C, Time 3.60e+6 sec | 70100 psi @Thickness 2.95 in, Temperature 212 °F, Time 1000 hour |
| 503 MPa @Treatment Temp. 24.0 °C, Thickness 75.0 mm | 73000 psi @Treatment Temp. 75.2 °F, Thickness 2.95 in |
| 97.0 MPa @Time 3.60e+7 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 14100 psi @Time 10000 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 103 MPa @Time 3.60e+6 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 14900 psi @Time 1000 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 110 MPa @Time 3.60e+7 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 16000 psi @Time 10000 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 138 MPa @Time 3.60e+6 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 20000 psi @Time 1000 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 145 MPa @Time 360000 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 21000 psi @Time 100 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 152 MPa @Time 3.60e+7 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 22000 psi @Time 10000 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 207 MPa @Time 360000 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 30000 psi @Time 100 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 228 MPa @Time 3.60e+6 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 33100 psi @Time 1000 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 228 MPa @Time 36000 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 33100 psi @Time 10.0 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 248 MPa @Time 3.60e+7 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 36000 psi @Time 10000 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 296 MPa @Time 36000 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 42900 psi @Time 10.0 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 331 MPa @Time 360000 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 48000 psi @Time 100 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 359 MPa @Time 3.60e+6 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 52100 psi @Time 1000 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 359 MPa @Time 1800 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 52100 psi @Time 0.500 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 427 MPa @Time 36000 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 61900 psi @Time 10.0 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 427 MPa @Time 1800 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 61900 psi @Time 0.500 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 441 MPa @Time 360 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 64000 psi @Time 0.100 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 462 MPa @Time 360000 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 67000 psi @Time 100 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 469 MPa @Time 360 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 68000 psi @Time 0.100 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 483 MPa @Time 1800 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 70100 psi @Time 0.500 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 490 MPa @Time 360 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 71100 psi @Time 0.100 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 496 MPa @Time 36000 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 71900 psi @Time 10.0 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 503 MPa @Time 360 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 73000 psi @Time 0.100 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 503 MPa @Time 1800 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 73000 psi @Time 0.500 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 503 MPa @Time 3.60e+7 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 73000 psi @Time 10000 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 503 MPa @Time 360 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 73000 psi @Time 0.100 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 503 MPa @Time 1800 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 73000 psi @Time 0.500 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 510 MPa @Time 36000 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 74000 psi @Time 10.0 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 510 MPa @Time 360000 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 74000 psi @Time 100 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 517 MPa @Time 3.60e+6 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 75000 psi @Time 1000 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
Elongation at Break | 12 % @Thickness 1.60 mm | 12 % @Thickness 0.0630 in |
| 12 % @Thickness 75.0 mm, Temperature -253 °C | 12 % @Thickness 2.95 in, Temperature -423 °F |
| 13 % @Thickness 75.0 mm, Temperature -196 °C | 13 % @Thickness 2.95 in, Temperature -321 °F |
| 14 % @Thickness 75.0 mm, Temperature -80.0 °C | 14 % @Thickness 2.95 in, Temperature -112 °F |
| 14 % @Thickness 75.0 mm, Temperature 24.0 °C | 14 % @Thickness 2.95 in, Temperature 75.2 °F |
| 16 % @Thickness 75.0 mm, Temperature -28.0 °C | 16 % @Thickness 2.95 in, Temperature -18.4 °F |
| 14 % @Time 360 sec, Thickness 75.0 mm, Temperature 100 °C | 14 % @Time 0.100 hour, Thickness 2.95 in, Temperature 212 °F |
| 15 % @Time 1800 sec, Thickness 75.0 mm, Temperature 100 °C | 15 % @Time 0.500 hour, Thickness 2.95 in, Temperature 212 °F |
| 16 % @Time 36000 sec, Thickness 75.0 mm, Temperature 100 °C | 16 % @Time 10.0 hour, Thickness 2.95 in, Temperature 212 °F |
| 16 % @Thickness 75.0 mm, Temperature 100 °C, Time 360000 sec | 16 % @Thickness 2.95 in, Temperature 212 °F, Time 100 hour |
| 17 % @Thickness 75.0 mm, Temperature 100 °C, Time 3.60e+6 sec | 17 % @Thickness 2.95 in, Temperature 212 °F, Time 1000 hour |
| 17 % @Thickness 75.0 mm, Temperature 100 °C, Time 3.60e+7 sec | 17 % @Thickness 2.95 in, Temperature 212 °F, Time 10000 hour |
| 18 % @Time 1800 sec, Thickness 75.0 mm, Temperature 149 °C | 18 % @Time 0.500 hour, Thickness 2.95 in, Temperature 300 °F |
| 20 % @Time 360 sec, Thickness 75.0 mm, Temperature 149 °C | 20 % @Time 0.100 hour, Thickness 2.95 in, Temperature 300 °F |
| 20 % @Time 36000 sec, Thickness 75.0 mm, Temperature 149 °C | 20 % @Time 10.0 hour, Thickness 2.95 in, Temperature 300 °F |
| 20 % @Time 360 sec, Thickness 75.0 mm, Temperature 176 °C | 20 % @Time 0.100 hour, Thickness 2.95 in, Temperature 349 °F |
| 20 % @Time 360 sec, Thickness 75.0 mm, Temperature 204 °C | 20 % @Time 0.100 hour, Thickness 2.95 in, Temperature 399 °F |
| 20 % @Time 360 sec, Thickness 75.0 mm, Temperature 232 °C | 20 % @Time 0.100 hour, Thickness 2.95 in, Temperature 450 °F |
| 25 % @Time 36000 sec, Thickness 75.0 mm, Temperature 176 °C | 25 % @Time 10.0 hour, Thickness 2.95 in, Temperature 349 °F |
| 25 % @Thickness 75.0 mm, Time 360000 sec, Temperature 176 °C | 25 % @Thickness 2.95 in, Time 100 hour, Temperature 349 °F |
| 25 % @Time 1800 sec, Thickness 75.0 mm, Temperature 232 °C | 25 % @Time 0.500 hour, Thickness 2.95 in, Temperature 450 °F |
| 25 % @Thickness 75.0 mm, Time 360000 sec, Temperature 149 °C | 25 % @Thickness 2.95 in, Time 100 hour, Temperature 300 °F |
| 25 % @Time 1800 sec, Thickness 75.0 mm, Temperature 176 °C | 25 % @Time 0.500 hour, Thickness 2.95 in, Temperature 349 °F |
| 30 % @Thickness 75.0 mm, Temperature 149 °C, Time 3.60e+6 sec | 30 % @Thickness 2.95 in, Temperature 300 °F, Time 1000 hour |
| 30 % @Thickness 75.0 mm, Temperature 149 °C, Time 3.60e+7 sec | 30 % @Thickness 2.95 in, Temperature 300 °F, Time 10000 hour |
| 30 % @Time 1800 sec, Thickness 75.0 mm, Temperature 204 °C | 30 % @Time 0.500 hour, Thickness 2.95 in, Temperature 399 °F |
| 35 % @Thickness 75.0 mm, Temperature 176 °C, Time 3.60e+6 sec | 35 % @Thickness 2.95 in, Temperature 349 °F, Time 1000 hour |
| 35 % @Time 36000 sec, Thickness 75.0 mm, Temperature 204 °C | 35 % @Time 10.0 hour, Thickness 2.95 in, Temperature 399 °F |
| 35 % @Thickness 75.0 mm, Time 360000 sec, Temperature 204 °C | 35 % @Thickness 2.95 in, Time 100 hour, Temperature 399 °F |
| 35 % @Time 36000 sec, Thickness 75.0 mm, Temperature 232 °C | 35 % @Time 10.0 hour, Thickness 2.95 in, Temperature 450 °F |
| 40 % @Thickness 75.0 mm, Time 360000 sec, Temperature 232 °C | 40 % @Thickness 2.95 in, Time 100 hour, Temperature 450 °F |
| 45 % @Thickness 75.0 mm, Temperature 204 °C, Time 3.60e+6 sec | 45 % @Thickness 2.95 in, Temperature 399 °F, Time 1000 hour |
| 45 % @Thickness 75.0 mm, Temperature 232 °C, Time 3.60e+6 sec | 45 % @Thickness 2.95 in, Temperature 450 °F, Time 1000 hour |
| 50 % @Thickness 75.0 mm, Temperature 232 °C, Time 3.60e+7 sec | 50 % @Thickness 2.95 in, Temperature 450 °F, Time 10000 hour |
| 55 % @Thickness 75.0 mm, Temperature 176 °C, Time 3.60e+7 sec | 55 % @Thickness 2.95 in, Temperature 349 °F, Time 10000 hour |
| 65 % @Thickness 75.0 mm, Temperature 204 °C, Time 3.60e+7 sec | 65 % @Thickness 2.95 in, Temperature 399 °F, Time 10000 hour |
| 14 % @Treatment Temp. 24.0 °C, Thickness 75.0 mm | 14 % @Treatment Temp. 75.2 °F, Thickness 2.95 in |
| 14 % @Time 360 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 14 % @Time 0.100 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 14 % @Time 1800 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 14 % @Time 0.500 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 14 % @Time 36000 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 14 % @Time 10.0 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 14 % @Time 360000 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 14 % @Time 100 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 14 % @Time 3.60e+6 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 14 % @Time 1000 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 14 % @Time 3.60e+7 sec, Treatment Temp. 100 °C, Thickness 75.0 mm | 14 % @Time 10000 hour, Treatment Temp. 212 °F, Thickness 2.95 in |
| 14 % @Time 360 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 14 % @Time 0.100 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 14 % @Time 1800 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 14 % @Time 0.500 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 14 % @Time 1800 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 14 % @Time 0.500 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 15 % @Time 360 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 15 % @Time 0.100 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 15 % @Time 1800 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 15 % @Time 0.500 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 15 % @Time 36000 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 15 % @Time 10.0 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 16 % @Time 360000 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 16 % @Time 100 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 16 % @Time 36000 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 16 % @Time 10.0 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 16 % @Time 360000 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 16 % @Time 100 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 16 % @Time 360 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 16 % @Time 0.100 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 16 % @Time 36000 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 16 % @Time 10.0 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 16 % @Time 360 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 16 % @Time 0.100 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 16 % @Time 1800 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 16 % @Time 0.500 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 17 % @Time 3.60e+6 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 17 % @Time 1000 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 17 % @Time 36000 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 17 % @Time 10.0 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 18 % @Time 3.60e+6 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 18 % @Time 1000 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 18 % @Time 360000 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 18 % @Time 100 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 18 % @Time 3.60e+7 sec, Treatment Temp. 149 °C, Thickness 75.0 mm | 18 % @Time 10000 hour, Treatment Temp. 300 °F, Thickness 2.95 in |
| 19 % @Time 360000 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 19 % @Time 100 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 20 % @Time 3.60e+7 sec, Treatment Temp. 176 °C, Thickness 75.0 mm | 20 % @Time 10000 hour, Treatment Temp. 349 °F, Thickness 2.95 in |
| 20 % @Time 3.60e+6 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 20 % @Time 1000 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 25 % @Time 3.60e+7 sec, Treatment Temp. 204 °C, Thickness 75.0 mm | 25 % @Time 10000 hour, Treatment Temp. 399 °F, Thickness 2.95 in |
| 25 % @Time 3.60e+6 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 25 % @Time 1000 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
| 25 % @Time 3.60e+7 sec, Treatment Temp. 232 °C, Thickness 75.0 mm | 25 % @Time 10000 hour, Treatment Temp. 450 °F, Thickness 2.95 in |
Tensile Modulus | 72.0 GPa | 10400 ksi |
Poissons Ratio | 0.33 | 0.33 |
Fatigue Strength | 160 MPa @# of Cycles 5.00e+8 | 23200 psi @# of Cycles 5.00e+8 |
Fracture Toughness | >= 23.1 MPa-m½ | >= 21.0 ksi-in½ |
| >= 23.1 MPa-m½ | >= 21.0 ksi-in½ |
| 26.4 MPa-m½ | 24.0 ksi-in½ |
| >= 27.5 MPa-m½ | >= 25.0 ksi-in½ |
| 28.6 MPa-m½ | 26.0 ksi-in½ |
| 29.7 MPa-m½ | 27.0 ksi-in½ |
| >= 29.7 MPa-m½ | >= 27.0 ksi-in½ |
| 31.0 MPa-m½ | 28.2 ksi-in½ |
| >= 33.0 MPa-m½ | >= 30.0 ksi-in½ |
| 33.0 MPa-m½ | 30.0 ksi-in½ |
| 34.0 MPa-m½ | 30.9 ksi-in½ |
| 37.4 MPa-m½ | 34.0 ksi-in½ |
| 38.0 MPa-m½ | 34.6 ksi-in½ |
Shear Modulus | 27.0 GPa | 3920 ksi |
Shear Strength | 326 MPa | 47300 psi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000430 ohm-cm | 0.00000430 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 21.6 µm/m-°C @Temperature -50.0 - 20.0 °C | 12.0 µin/in-°F @Temperature -58.0 - 68.0 °F |
| 23.4 µm/m-°C @Temperature 20.0 - 100 °C | 13.0 µin/in-°F @Temperature 68.0 - 212 °F |
| 24.3 µm/m-°C @Temperature 20.0 - 200 °C | 13.5 µin/in-°F @Temperature 68.0 - 392 °F |
| 25.2 µm/m-°C @Temperature 20.0 - 300 °C | 14.0 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.864 J/g-°C | 0.207 BTU/lb-°F |
Thermal Conductivity | 155 W/m-K | 1080 BTU-in/hr-ft²-°F |
Melting Point | 477 - 635.0 °C | 890 - 1175 °F |
Solidus | 477 °C | 890 °F |
Liquidus | 635.0 °C | 1175 °F |
|
Processing Properties | Metric | English | Comments |
---|
Annealing Temperature | 413 °C | 775 °F |
Solution Temperature | 516 °C | 960 °F |
Aging Temperature | 121 - 177 °C | 250 - 350 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 88 - 91.4 % | 88 - 91.4 % |
Chromium, Cr | 0.18 - 0.28 % | 0.18 - 0.28 % |
Copper, Cu | 1.2 - 2.0 % | 1.2 - 2.0 % |
Iron, Fe | <= 0.20 % | <= 0.20 % |
Magnesium, Mg | 2.1 - 2.9 % | 2.1 - 2.9 % |
Manganese, Mn | <= 0.10 % | <= 0.10 % |
Other, each | <= 0.05 % | <= 0.05 % |
Other, total | <= 0.15 % | <= 0.15 % |
Silicon, Si | <= 0.15 % | <= 0.15 % |
Titanium, Ti | <= 0.10 % | <= 0.10 % |
Zinc, Zn | 5.1 - 6.1 % | 5.1 - 6.1 % |