MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Equate EFDC-7050 LLDPE Film Extrusion Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade

Material Notes: EFDC-7050 is a linear low-density polyethylene resin for tubular blown film extrusion. Films extruded from EFDC-7050 have good toughness and high tensile strength and puncture resistance. The product offers excellent draw down capability for making thinner gauge films. EFDC-7050 contains high levels of slip and antiblocking agent. It offers excellent sealing and machining characteristics for high-speed film converting operations

Applications: EFDC-7050 is recommended for the manufacture of thin gauge liner films, garment bags and films for other industrial, food packaging and other general-purpose applications requiring toughness and puncture resistance.

Information provided by Equate

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.530 g/cc0.0191 lb/in³ASTM D1895
Density 0.918 g/cc0.0332 lb/in³ASTM D792
Thickness 25.0 microns0.984 milAs Tested
Melt Flow 2.0 g/10 min
@Load 2.16 kg
2.0 g/10 min
@Load 4.76 lb
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Elmendorf Tear Strength, MD 31.0 g/micron
@Thickness 0.0250 mm
787 g/mil
@Thickness 0.000984 in
ASTM D1922
Elmendorf Tear Strength, TD 124 g/micron
@Thickness 0.0250 mm
3150 g/mil
@Thickness 0.000984 in
ASTM D1922
Dart Drop 3.60 g/micron
@Thickness 0.0250 mm
91.4 g/mil
@Thickness 0.000984 in
ASTM D1709 A
Dart Drop Test 90.0 g0.198 lbF50; ASTM D1709 A
Film Tensile Strength at Break, MD 31.0 MPa
@Thickness 0.0250 mm
4500 psi
@Thickness 0.000984 in
ASTM D882
Film Tensile Strength at Break, TD 23.0 MPa
@Thickness 0.0250 mm
3340 psi
@Thickness 0.000984 in
ASTM D882
1% Secant Modulus, MD 195 MPa
@Thickness 0.0250 mm
28300 psi
@Thickness 0.000984 in
ASTM D882
1% Secant Modulus, TD 220 MPa
@Thickness 0.0250 mm
31900 psi
@Thickness 0.000984 in
ASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 124 °C255 °FEquate Test Method
 
Optical PropertiesMetricEnglishComments
Haze 13 %13 %ASTM D1003
Gloss 55 %55 %45°; ASTM D2457
 
Processing PropertiesMetricEnglishComments
Zone 1 170 °C338 °F
Zone 2 180 °C356 °F
Zone 3 185 °C365 °F
Zone 4 180 °C356 °F
Adapter Temperature 180 °C356 °F
Die Temperature 180 °C356 °F
Melt Temperature 180 °C356 °F
Head Temperature 180 °C356 °F
Die Opening >= 0.180 cm>= 0.0709 in
Blow-up Ratio (BUR) 2.02.02:1 As Tested
 
Descriptive Properties
Puncture Energy60 J/mmEquate Test Method

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Equate EFDC-7087 LLDPE Film Extrusion Resin
Equate EFDA-7047 LLDPE Film Extrusion Resin
Equate EGDA-6888 HDPE Film Extrusion Resin
Versalis Flexirene® MR 50 U Linear Low Density Polyethylene
Borealis Borstar® FB2310 LLDPE for Film

PEQUAT907 / 150435

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.