MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

KBI® 10 Tantalum Alloy (UNS R05255)
Categories: Metal; Nonferrous Metal; Refractory Metal

Material Notes: Ta-10W (electron-beam cast)

Key Words: UNS R05255
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 16.9 g/cc0.611 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 245245
Tensile Strength 345 MPa
@Temperature 1320 °C
50000 psi
@Temperature 2400 °F
Recrystallized
Tensile Strength, Ultimate 550 - 620 MPa79800 - 89900 psi
Tensile Strength, Yield 460 - 482 MPa
@Strain 0.2 %
66700 - 69900 psi
@Strain 0.2 %
Elongation at Break 30 %30 %
Rupture Strength 138 MPa
@Temperature 1320 °C,
Time 36000 sec
20000 psi
@Temperature 2400 °F,
Time 10.0 hour
Recrystallized
Modulus of Elasticity 205 - 207 GPa29700 - 30000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000176 ohm-cm0.0000176 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Melting Point 3030 °C5490 °F
 
Component Elements PropertiesMetricEnglishComments
Tantalum, Ta 90 %90 %As balance
Tungsten, W 10 %10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Cabot 10 Tantalum Alloy (UNS R05255)
Tantaloy® 60 Tantalum Alloy (UNS R05255)
Tantaloy® 63 (FS63) Tantalum Alloy (UNS R05252)
KBI® 40 Tantalum Alloy (UNS R05240)
KBI® 2 Tantalum Alloy (UNS R05252)

MRTa05 / 100355

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.