MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

RTP Company RTP 301 HF FR Polycarbonate (PC), High Flow - Glass Fiber - Flame Retardant - Non-PBBO/E - UL94 V-0
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Glass Fiber Filled, Flame Retardant

Material Notes: The RTP series of flame retardant, glass fiber reinforced polycarbonate materials offer dimensional stability with improved heat distortion and ignition reisstance performance over the base resin. RTP 301 HF FR is a special low viscosity grade.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.28 g/cc1.28 g/ccASTM D 792
Filler Content 10 %10 %Primary Additive
Water Absorption 0.10 %0.10 %24 hrs @ 23°C; ASTM D 570
Linear Mold Shrinkage 0.0030 - 0.0050 cm/cm
@Thickness 3.17 mm
0.0030 - 0.0050 in/in
@Thickness 0.125 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 55.2 MPa8000 psiASTM D 638
Elongation at Break >= 10 %>= 10 %ASTM D 638
Tensile Modulus 3.10 GPa450 ksiASTM D 638
Flexural Strength 100 MPa14500 psiASTM D 790
Flexural Modulus 3.10 GPa450 ksiASTM D 790
Izod Impact, Notched 0.961 J/cm
@Thickness 3.17 mm
1.80 ft-lb/in
@Thickness 0.125 in
D 256
Izod Impact, Unnotched NB
@Thickness 3.17 mm
NB
@Thickness 0.125 in
ASTM D4812
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmASTM D 257
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 146 °C295 °FASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 138 °C280 °FASTM D 648
Flammability, UL94 V-0
@Thickness 1.59 mm
V-0
@Thickness 0.0625 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 288 - 316 °C550 - 600 °F
Mold Temperature 82.2 - 121 °C180 - 250 °F
Drying Temperature 121 °C250 °F
Dry Time 4 hour4 hour
Moisture Content 0.020 %0.020 %
Dew Point -28.9 °C-20.0 °F
Injection Pressure 68.9 - 103 MPa10000 - 15000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RTP Company RTP 305 FR UV Polycarbonate (PC), Glass Fiber - Flame Retardant - Non-PBBO/E - UV Stabilized
RTP Company RTP 303 FR UV Polycarbonate (PC), Glass Fiber - Flame Retardant - Non-PBBO/E - UV Stabilized
RTP Company RTP 301-500 Polycarbonate (PC), Glass Fiber - Flame Retardant - Non-PBBO/E - UL94 V-0

PQZWA1148 / 90617

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.