MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil Geolast® 701-87W183 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: A hard, black, oil resistant thermoplastic vulcanizate (TPV) in the thermoplastic elastomer (TPE) family. This material combines good hot air and hot oil resistance for use in a wide range of applications. This grade of Geolast TPV is shear-dependent and can be processed on conventional thermoplastics equipment for injection molding, extrusion or blow molding. It is polyolefin based and completely recyclable.

Recyclable. Designed for improved fluid resistance.

Information provided by ExxonMobil and predecessor Advanced Elastomer Systems.

Key Words: EU 2003/11/EC; RoHS Compliant
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.02 g/cc0.0368 lb/in³ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 8282After Aging: Air at 257°F, 168 hr; ASTM D573
 87
@Time 15.0 sec
87
@Time 0.00417 hour
ISO 868
Tensile Strength at Break 7.4967 MPa1087.3 psiAfter Aging: 257°F, 70 hr in IRM 903 Oil; ASTM D471
 8.41 MPa1220 psiAcross Flow; ASTM D412
 10.387 MPa1506.5 psiAfter Aging: Air at 257°F, 168 hr; ASTM D573
Elongation at Break 227.7 %227.7 %After Aging: 257°F, 70 hr in IRM 903 Oil; ASTM D471
 244.2 %244.2 %After Aging: Air at 257°F, 168 hr; ASTM D573
 280 %280 %Across Flow; ASTM D412
100% Modulus 4.90 MPa
@Strain 100 %
711 psi
@Strain 100 %
Across Flow; ASTM D412
Tear Strength 30.0 kN/m171 pliDie C- Across Flow; ASTM D624
Compression Set  38 %
@Temperature 70.0 °C,
Time 79200 sec
38 %
@Temperature 158 °F,
Time 22.0 hour
Type 1; ASTM D395B
 55 %
@Temperature 125 °C,
Time 252000 sec
55 %
@Temperature 257 °F,
Time 70.0 hour
Type 1; ASTM D395B
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -32.8 °C-27.0 °FASTM D746
 
Processing PropertiesMetricEnglishComments
Processing Temperature 175 - 230 °C347 - 446 °F
Melt Temperature <= 102 °C<= 215 °F
 
Descriptive Properties
Change in Mass in IRM 903 Oil at 257°F for 70 hr0.48
ColorBlack
FormPellets

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil Geolast® 701-70 Thermoplastic Elastomer
ExxonMobil Geolast® 701-80W183 Thermoplastic Elastomer
ExxonMobil Geolast® 703-45 Thermoplastic Elastomer
ExxonMobil Santoprene® 171-73 Thermoplastic Elastomer
ExxonMobil Vyram™ 9101-85 Thermoplastic Elastomer

PADVA036 / 22726

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.