  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Trinseo PULSE™ B-270 PC/ABS
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: Engineering Resin

Information provided by Trinseo.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.21 g/cc0.0437 lb/in³ASTM D792
Water Absorption 0.050 %
@Temperature 23.0 °C,
Time 86400 sec
0.050 %
@Temperature 73.4 °F,
Time 24.0 hour
ASTM D570
Moisture Absorption at Equilibrium 0.18 %0.18 %ASTM D570
Melt Flow 1.5 g/10 min
@Load 3.80 kg,
Temperature 230 °C
1.5 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 51.4 MPa7450 psiASTM D638
Tensile Strength, Yield 59.9 MPa8690 psiASTM D638
Elongation at Break 100 %100 %ASTM D638
Flexural Yield Strength 100 MPa14500 psiASTM D790
Flexural Modulus 3.31 GPa480 ksiASTM D790
Izod Impact, Notched  1.10 J/cm
@Thickness 3.20 mm,
Temperature -29.0 °C
2.06 ft-lb/in
@Thickness 0.126 in,
Temperature -20.2 °F
ASTM D256
 3.70 J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
6.93 ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
Dart Drop, Total Energy  56.5 J
@Thickness 3.20 mm,
Temperature -29.0 °C
41.7 ft-lb
@Thickness 0.126 in,
Temperature -20.2 °F
ASTM D3763
 56.5 J
@Thickness 3.20 mm,
Temperature 23.0 °C
41.7 ft-lb
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Transverse to Flow 63.0 µm/m-°C35.0 µin/in-°FASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 134 °C
@Thickness 3.20 mm
273 °F
@Thickness 0.126 in
Unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Melt Temperature 277 - 293 °C531 - 559 °F
Mold Temperature 71.0 - 93.0 °C160 - 199 °F
Drying Temperature 99.0 °C210 °F
Dry Time 4.00 hour4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
Schott B270™ Sheet Glass
Covestro Bayblend® FR3000 PC/ABS Blend
Versalis KOBLEND PCA PD 54 PC+ABS
Versalis KOBLEND PCA PD 935 G2 PC+ABS, 10% Glass Fiber

PDOW1407 / 30625

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.