MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Kolon KOPA® KN333HI5BL High Impact Nylon 66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Impact Grade

Material Notes: Middle viscosity, Impact -resistant

Applications A variety of fuse boxes, relax boxes

Information provided by API-Kolon.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.10 g/cc1.10 g/ccASTM D792
Moisture Absorption at Equilibrium 1.0 %1.0 %60% RH; ASTM D570
Linear Mold Shrinkage 0.016 - 0.019 cm/cm0.016 - 0.019 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 110110ASTM D785
Tensile Strength 59.0 MPa8560 psiASTM D638
Elongation at Break 50 %50 %ASTM D638
Flexural Strength 88.0 MPa12800 psiASTM D790
Flexural Modulus 2.256 GPa327.2 ksiASTM D790
Izod Impact, Notched 4.90 J/cm9.18 ft-lb/inASTM D256
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 3.13.1ASTM D150
Dielectric Strength 20.0 kV/mm508 kV/inASTM D149
Arc Resistance 125 sec125 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear 60.0 µm/m-°C33.3 µin/in-°FASTM D696
Melting Point 255 °C491 °FASTM D1525
Deflection Temperature at 0.46 MPa (66 psi) 210 °C410 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 70.0 °C158 °FASTM D648
Flammability, UL94 HBHB

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Kolon KOPA® KN3321G10V0L G/F Reinforced & Flame Retardant Nylon 66
Kolon KOPA® KN333C22 CF Reinforced Nylon 66
Kolon KOPA® KN333G30BL G/F Reinforced Nylon 66
Kolon KOPA® KN333G45 G/F Reinforced Nylon 66
Kolon KOPA® KN333NW High Impact Nylon 66

PKOKZ946 / 122648

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.