MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Mitsubishi Hostaphan® WN, 350 micron Nominal Thickness Translucent White Polyethylene Terephthalate Film
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), Unreinforced

Material Notes: Hostaphan® WN is a white film made of polyethylene terephthalate (PET) and is well suited for electrical insulating of machines and appliances. The high dielectric strength and large volume resistance of Hostaphan® WN make it possible to use the film as a high-quality insulation material.

Applications:

  • Insulation of winding heads
  • Single phase insulation
  • Slot insulation
  • Ballasts

Information provided by Mitsubishi Polyester Film

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Linear Mold Shrinkage 0.010 cm/cm
@Time 900 sec
0.010 in/in
@Time 0.250 hour
DIN 40634
Linear Mold Shrinkage, Transverse 0.010 cm/cm
@Time 900 sec
0.010 in/in
@Time 0.250 hour
DIN 40634
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 160 MPa23200 psiTest speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Film Tensile Strength at Yield, TD 180 MPa26100 psiTest speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Film Elongation at Break, MD >= 230 %>= 230 %Test speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
Film Elongation at Break, TD 170 %170 %Test speed 100%/min.; 50% r.h.; ISO 527-1, ISO 527-3; Sample type 2
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant  3.3
@Frequency 50 Hz,
Temperature 23.0 °C
3.3
@Frequency 50 Hz,
Temperature 73.4 °F
DIN 40634 or VDE 0345 in air or ASTM D150
 3.3
@Frequency 1000 Hz,
Temperature 23.0 °C
3.3
@Frequency 1000 Hz,
Temperature 73.4 °F
DIN 40634 or VDE 0345 in air or ASTM D150
 3.6
@Frequency 50 Hz,
Temperature 150 °C
3.6
@Frequency 50 Hz,
Temperature 302 °F
DIN 40634 or VDE 0345 in air or ASTM D150
Dissipation Factor  0.0020
@Frequency 50 Hz,
Temperature 23.0 °C
0.0020
@Frequency 50 Hz,
Temperature 73.4 °F
DIN 40634 or VDE 0345 in air or ASTM D149
 0.0048
@Frequency 50 Hz,
Temperature 150 °C
0.0048
@Frequency 50 Hz,
Temperature 302 °F
DIN 40634 or VDE 0345 in air or ASTM D149
 0.0052
@Frequency 1000 Hz,
Temperature 23.0 °C
0.0052
@Frequency 1000 Hz,
Temperature 73.4 °F
DIN 40634 or VDE 0345 in air or ASTM D149
 
Descriptive Properties
Behavior Under the Influence of Partial Discharges (Min.)900DIN 53485 or VDE 0303/part 7; Contact method, 40KV/mm
Conductivity of Aqueous Extract (µS/cm)2DIN 40634 or VDE 0345; 1 kHz
Frigen Extract (%)0.05DIN 8944; Cold extraction
Insulation Class in Electrical EngineeringBDIN 57530 or VDE 0530, main list
Trichloroethylene- Extract (%)0.2DIN 8943; Extracted in Soxhalet apparatus for 2h. Boiled down for 15h at 105ºC

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Mitsubishi Hostaphan® RN, 15 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Mitsubishi Hostaphan® RN, 50 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Mitsubishi Hostaphan® RN, 12 micron Nominal Thickness Universal Polyethylene Terephthalate Film
Armacell ArmaForm® PET Foil 70
Mitsubishi Hostaphan® RN, 100 micron Nominal Thickness Universal Polyethylene Terephthalate Film

PMUE043 / 108424

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.