MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

BorsodChem ONGRO CPE 3602 C Chlorinated Polyethylene
Categories: Other Engineering Material; Additive/Filler for Polymer; Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: IMPACT MODIFIER FOR PVC
  • high impact resistance
  • good processability
  • excellent weather resistance

ELASTOMERS

  • variety of cross-linking technologies
  • excellent ozone- and weather resistance
  • excellent chemical resistance
  • good electrical properties
  • freely colorable

PLASTIC MATERIALS, FLAME RETARDANT ADDITIVE

  • compatibility with a large number of polymers
  • simple mixing
  • outstanding heat stability
  • excellent weather resistance
  • low flammability
  • plasticizer free flexible systems

Information provided by BorsodChem Rt.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Apparent Bulk Density 0.460 g/cc0.0166 lb/in³MSZ ISO 60
Particle Size 600 µm600 µm<1% above
Viscosity 2.50e+6 cP
@Shear Rate 200 1/s,
Temperature 190 °C
2.50e+6 cP
@Shear Rate 200 1/s,
Temperature 374 °F
Capillary viscosimeter
Mooney Viscosity 70
@Temperature 120 °C
70
@Temperature 248 °F
ML(1+4); MSZ 11093 ISO 289
Crystallinity <= 1.0 %<= 1.0 %Residual; DSC BC HSz 325
Collected Volatile Condensable Material <= 0.30 %<= 0.30 %ISO 1269
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6060MSZ ISO 868
Tensile Strength at Break 14.0 MPa2030 psiMSZ ISO 527
Elongation at Break 600 %600 %MSZ ISO 527
100% Modulus 1.20 MPa
@Strain 100 %
174 psi
@Strain 100 %
MSZ ISO 527
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 4.50 °C40.1 °FDMA method 1 Hz
 
Descriptive Properties
Chlorine Content, %36
Heat Stability at 180°C, minutes8

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BorsodChem ONGRO CPE 4002 N Chlorinated Polyethylene
Avient FireCon™ CPE-37-11 RoHS Black Polyethylene, Chlorinated (CPE)
Avient FireCon™ CPE 1240 UV RoHS NATURAL Polyethylene, Chlorinated (CPE)
Avient FireCon™ CPE 37-11 RoHS BLACK Polyethylene, Chlorinated (CPE)
Avient FireCon™ CPE 32-33 RoHS Black Polyethylene, Chlorinated (CPE)

PBORS18 / 27542

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.