MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Overview of materials for Nylon 6, Unreinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.670 - 4.50 g/cc0.0242 - 0.163 lb/in³Average value: 1.14 g/cc Grade Count:816
Water Absorption 0.100 - 11.0 %0.100 - 11.0 %Average value: 4.51 % Grade Count:337
Moisture Absorption at Equilibrium 0.0400 - 9.50 %0.0400 - 9.50 %Average value: 2.82 % Grade Count:340
 1.60 - 1.65 %
@Temperature 70.0 - 70.0 °C
1.60 - 1.65 %
@Temperature 158 - 158 °F
Average value: 1.63 % Grade Count:12
Water Absorption at Saturation 1.70 - 10.0 %1.70 - 10.0 %Average value: 8.57 % Grade Count:175
Particle Size 10.0 - 80.0 µm10.0 - 80.0 µmAverage value: 50.0 µm Grade Count:5
Oxygen Transmission Rate 40.3 cc/m²/day2.60 cc/100 in²/dayAverage value: 40.3 cc/m²/day Grade Count:10
Nitrogen Transmission 14.0 cc-mm/m²-24hr-atm35.6 cc-mil/100 in²-24hr-atmAverage value: 14.0 cc-mm/m²-24hr-atm Grade Count:10
Carbon Dioxide Transmission 72.8 - 250 cc-mm/m²-24hr-atm185 - 635 cc-mil/100 in²-24hr-atmAverage value: 88.2 cc-mm/m²-24hr-atm Grade Count:11
Viscosity 2.60 - 50.0 cP2.60 - 50.0 cPAverage value: 7.64 cP Grade Count:25
 258 - 350000 cP
@Temperature 200 - 290 °C
258 - 350000 cP
@Temperature 392 - 554 °F
Average value: 98800 cP Grade Count:3
 258 - 350000 cP
@Shear Rate 0.100 - 1000 1/s
258 - 350000 cP
@Shear Rate 0.100 - 1000 1/s
Average value: 98800 cP Grade Count:3
Viscosity Test 150 - 263 cm³/g1.50 - 2.63 dl/gAverage value: 202 cm³/g Grade Count:8
Viscosity Number 118 - 450 cm³/g1.18 - 4.50 dl/gAverage value: 192 cm³/g Grade Count:49
Maximum Moisture Content 0.0200 - 0.2000.0200 - 0.200Average value: 0.156 Grade Count:29
Linear Mold Shrinkage 0.00190 - 0.0508 cm/cm0.00190 - 0.0508 in/inAverage value: 0.0128 cm/cm Grade Count:428
 0.0100 - 0.0100 cm/cm
@Temperature 80.0 - 80.0 °C
0.0100 - 0.0100 in/in
@Temperature 176 - 176 °F
Average value: 0.0100 cm/cm Grade Count:2
Linear Mold Shrinkage, Transverse 0.00110 - 0.108 cm/cm0.00110 - 0.108 in/inAverage value: 0.0128 cm/cm Grade Count:179
 0.0130 - 0.0130 cm/cm
@Temperature 80.0 - 80.0 °C
0.0130 - 0.0130 in/in
@Temperature 176 - 176 °F
Average value: 0.0130 cm/cm Grade Count:2
Melt Flow 1.00 - 198 g/10 min1.00 - 198 g/10 minAverage value: 42.9 g/10 min Grade Count:101
Spiral Flow 55.0 - 230 cm21.7 - 90.6 inAverage value: 84.9 cm Grade Count:7
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 82.0 - 88.082.0 - 88.0Average value: 85.0 Grade Count:8
Hardness, Rockwell R 73.0 - 12273.0 - 122Average value: 113 Grade Count:121
 80.0 - 83.0
@Temperature 80.0 - 80.0 °C
80.0 - 83.0
@Temperature 176 - 176 °F
Average value: 80.6 Grade Count:5
Hardness, H358/30 70.0 - 160 MPa10200 - 23200 psiAverage value: 118 MPa Grade Count:4
Hardness, Shore D 57.0 - 87.057.0 - 87.0Average value: 77.3 Grade Count:46
Hardness, Shore M 48.0 - 80.048.0 - 80.0Average value: 74.7 Grade Count:6
Ball Indentation Hardness 30.0 - 190 MPa4350 - 27600 psiAverage value: 103 MPa Grade Count:76
Tensile Strength, Ultimate 10.0 - 225 MPa1450 - 32600 psiAverage value: 67.0 MPa Grade Count:323
 18.0 - 195 MPa
@Temperature -40.0 - 120 °C
2610 - 28300 psi
@Temperature -40.0 - 248 °F
Average value: 52.4 MPa Grade Count:16
 10.0 - 100 MPa
@Temperature -20.0 - 100 °C
1450 - 14500 psi
@Temperature -4.00 - 212 °F
Average value: 52.4 MPa Grade Count:3
 10.0 - 100 MPa
@Strain 0.750 - 5.00 %
1450 - 14500 psi
@Strain 0.750 - 5.00 %
Average value: 52.4 MPa Grade Count:3
Tensile Strength, Yield 3.45 - 105 MPa500 - 15200 psiAverage value: 63.8 MPa Grade Count:458
 20.0 - 142 MPa
@Temperature -40.0 - 121 °C
2900 - 20600 psi
@Temperature -40.0 - 250 °F
Average value: 74.0 MPa Grade Count:16
Film Elongation at Break, TD 290 - 700 %290 - 700 %Average value: 493 % Grade Count:3
Elongation at Break 0.400 - 500 %0.400 - 500 %Average value: 64.0 % Grade Count:626
 1.00 - 57.0 %
@Temperature -40.0 - 80.0 °C
1.00 - 57.0 %
@Temperature -40.0 - 176 °F
Average value: 22.3 % Grade Count:9
Elongation at Yield 1.50 - 200 %1.50 - 200 %Average value: 14.7 % Grade Count:297
 3.00 - 42.0 %
@Temperature -40.0 - 121 °C
3.00 - 42.0 %
@Temperature -40.0 - 250 °F
Average value: 34.3 % Grade Count:5
Modulus of Elasticity 0.210 - 17.0 GPa30.5 - 2470 ksiAverage value: 2.64 GPa Grade Count:465
 0.360 - 3.75 GPa
@Temperature -40.0 - 120 °C
52.2 - 544 ksi
@Temperature -40.0 - 248 °F
Average value: 1.39 GPa Grade Count:8
Flexural Yield Strength 7.00 - 220 MPa1020 - 31900 psiAverage value: 81.0 MPa Grade Count:444
 8.00 - 270 MPa
@Temperature -40.0 - 250 °C
1160 - 39200 psi
@Temperature -40.0 - 482 °F
Average value: 89.4 MPa Grade Count:23
Flexural Modulus 0.100 - 13.7 GPa14.5 - 1990 ksiAverage value: 2.38 GPa Grade Count:525
 0.260 - 6.20 GPa
@Temperature -40.0 - 121 °C
37.7 - 899 ksi
@Temperature -40.0 - 250 °F
Average value: 1.71 GPa Grade Count:21
Flexural Strain at Break 1.10 - 9.00 %1.10 - 9.00 %Average value: 6.74 % Grade Count:56
Compressive Yield Strength 6.00 - 107 MPa870 - 15500 psiAverage value: 66.6 MPa Grade Count:17
Compressive Modulus 2.07 - 2.48 GPa300 - 360 ksiAverage value: 2.32 GPa Grade Count:3
Poissons Ratio 0.230 - 0.4500.230 - 0.450Average value: 0.349 Grade Count:7
Shear Strength 55.2 - 75.0 MPa8000 - 10900 psiAverage value: 68.8 MPa Grade Count:8
Secant Modulus 0.200 - 2.55 GPa29.0 - 370 ksiAverage value: 1.49 GPa Grade Count:3
 2.50 - 13.0 GPa
@Temperature -40.0 - 50.0 °C
363 - 1890 ksi
@Temperature -40.0 - 122 °F
Average value: 2.45 GPa Grade Count:2
 2.50 - 13.0 GPa
@Strain 0.000 - 20.0 %
363 - 1890 ksi
@Strain 0.000 - 20.0 %
Average value: 2.45 GPa Grade Count:2
Secant Modulus, TD 0.650 - 0.652 GPa94.3 - 94.6 ksiAverage value: 0.651 GPa Grade Count:3
Izod Impact, Notched 0.300 J/cm - NB0.562 ft-lb/in - NBAverage value: 1.47 J/cm Grade Count:252
 0.210 - 2.93645 J/cm
@Temperature -40.0 - -5.00 °C
0.393 - 5.50117 ft-lb/in
@Temperature -40.0 - 23.0 °F
Average value: 0.823 J/cm Grade Count:22
 0.534 - 2.54973 J/cm
@Temperature -40.0 - -30.0 °C
1.00 - 4.77669 ft-lb/in
@Temperature -40.0 - -22.0 °F
Average value: 0.823 J/cm Grade Count:4
 0.534 - 2.54973 J/cm
@Thickness 1.57 - 6.40 mm
1.00 - 4.77669 ft-lb/in
@Thickness 0.0618 - 0.252 in
Average value: 0.823 J/cm Grade Count:4
Izod Impact, Unnotched 0.587 J/cm - NB1.10 ft-lb/in - NBAverage value: 4.58 J/cm Grade Count:9
Izod Impact, Notched (ISO) 2.40 - 21000 kJ/m²1.14 - 9990 ft-lb/in²Average value: 24.6 kJ/m² Grade Count:163
 4.00 kJ/m² - NB
@Temperature -40.0 - -20.0 °C
1.90 ft-lb/in² - NB
@Temperature -40.0 - -4.00 °F
Average value: 15.0 kJ/m² Grade Count:65
Izod Impact, Unnotched (ISO) 4.50 - 21000 kJ/m²2.14 - 9990 ft-lb/in²Average value: 36.5 kJ/m² Grade Count:45
 65.0 kJ/m² - NB
@Temperature -30.0 - -30.0 °C
30.9 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Average value: 105 kJ/m² Grade Count:34
Charpy Impact Unnotched 0.320 J/cm² - NB1.52 ft-lb/in² - NBAverage value: 11.2 J/cm² Grade Count:340
 0.550 J/cm² - NB
@Temperature -40.0 - -20.0 °C
2.62 ft-lb/in² - NB
@Temperature -40.0 - -4.00 °F
Average value: 9.81 J/cm² Grade Count:179
Charpy Impact, Notched 0.110 J/cm² - NB0.524 ft-lb/in² - NBAverage value: 2.33 J/cm² Grade Count:371
 0.150 J/cm² - NB
@Temperature -40.0 - -20.0 °C
0.714 ft-lb/in² - NB
@Temperature -40.0 - -4.00 °F
Average value: 1.14 J/cm² Grade Count:171
Gardner Impact 1.36 - 36.2 J1.00 - 26.7 ft-lbAverage value: 25.0 J Grade Count:8
Dart Drop, Total Energy 67.8 - 285 J50.0 - 210 ft-lbAverage value: 204 J Grade Count:4
Puncture Energy 12.0 - 165 J8.85 - 122 ft-lbAverage value: 92.3 J Grade Count:12
 10.0 - 160 J
@Temperature -30.0 - -30.0 °C
7.38 - 118 ft-lb
@Temperature -22.0 - -22.0 °F
Average value: 77.3 J Grade Count:9
Coefficient of Friction 0.100 - 0.4200.100 - 0.420Average value: 0.239 Grade Count:27
Coefficient of Friction, Static 0.210 - 0.2500.210 - 0.250Average value: 0.222 Grade Count:4
Tensile Creep Modulus, 1 hour 700 - 3700 MPa102000 - 537000 psiAverage value: 1460 MPa Grade Count:7
Tensile Creep Modulus, 1000 hours 520 - 2900 MPa75400 - 421000 psiAverage value: 1150 MPa Grade Count:18
Elmendorf Tear Strength, TD 2.20 g/micron56.0 g/milAverage value: 2.20 g/micron Grade Count:3
K (wear) Factor 8.10 - 403 x 10-8 mm³/N-M4.02 - 200 x 10-10 in³-min/ft-lb-hrAverage value: 245 x 10-8 mm³/N-M Grade Count:5
Taber Abrasion, mg/1000 Cycles 3.00 - 12.03.00 - 12.0Average value: 4.90 Grade Count:10
Film Tensile Strength at Break, TD 41.0 - 90.3 MPa5950 - 13100 psiAverage value: 63.8 MPa Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0200 - 1.00e+18 ohm-cm0.0200 - 1.00e+18 ohm-cmAverage value: 4.26e+15 ohm-cm Grade Count:307
Surface Resistance 100 - 1.00e+16 ohm100 - 1.00e+16 ohmAverage value: 2.39e+14 ohm Grade Count:211
Dielectric Constant 2.80 - 20.02.80 - 20.0Average value: 5.03 Grade Count:208
Dielectric Strength 7.87 - 100 kV/mm200 - 2540 kV/inAverage value: 30.3 kV/mm Grade Count:208
Dissipation Factor 0.00500 - 0.3900.00500 - 0.390Average value: 0.0764 Grade Count:137
Dielectric Loss Index 0.0100 - 0.3000.0100 - 0.300Average value: 0.111 Grade Count:19
Arc Resistance 80.0 - 195 sec80.0 - 195 secAverage value: 136 sec Grade Count:26
Comparative Tracking Index 0.000 - 600 V0.000 - 600 VAverage value: 588 V Grade Count:181
Hot Wire Ignition, HWI 7.00 - 60.0 sec7.00 - 60.0 secAverage value: 28.4 sec Grade Count:5
High Amp Arc Ignition, HAI 120 arcs120 arcsAverage value: 120 arcs Grade Count:5
High Voltage Arc-Tracking Rate, HVTR 0.000 - 50.0 mm/min0.000 - 1.97 in/minAverage value: 16.6 mm/min Grade Count:5
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.00 - 200 µm/m-°C3.89 - 111 µin/in-°FAverage value: 80.5 µm/m-°C Grade Count:204
CTE, linear, Transverse to Flow 10.0 - 200 µm/m-°C5.56 - 111 µin/in-°FAverage value: 102 µm/m-°C Grade Count:65
Specific Heat Capacity 1.20 - 3.05 J/g-°C0.287 - 0.730 BTU/lb-°FAverage value: 1.71 J/g-°C Grade Count:42
Thermal Conductivity 0.230 - 31.7 W/m-K1.60 - 220 BTU-in/hr-ft²-°FAverage value: 2.89 W/m-K Grade Count:64
Melting Point 141 - 315 °C286 - 599 °FAverage value: 220 °C Grade Count:604
Crystallization Temperature 149 - 174 °C300 - 345 °FAverage value: 165 °C Grade Count:3
Maximum Service Temperature, Air 65.0 - 250 °C149 - 482 °FAverage value: 122 °C Grade Count:108
Hot Ball Pressure Test 125 - 165 °C257 - 329 °FAverage value: 145 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 53.0 - 256 °C127 - 493 °FAverage value: 166 °C Grade Count:310
Deflection Temperature at 1.8 MPa (264 psi) 32.2 - 225 °C90.0 - 437 °FAverage value: 71.3 °C Grade Count:503
Deflection Temperature at 8.0 MPa 40.0 - 55.0 °C104 - 131 °FAverage value: 43.7 °C Grade Count:20
Vicat Softening Point 70.0 - 302 °C158 - 576 °FAverage value: 193 °C Grade Count:144
Heat Distortion Temperature 180 - 240 °C356 - 464 °FAverage value: 220 °C Grade Count:4
Minimum Service Temperature, Air -60.0 - -10.0 °C-76.0 - 14.0 °FAverage value: -37.9 °C Grade Count:43
Glass Transition Temp, Tg 60.0 - 160 °C140 - 320 °FAverage value: 120 °C Grade Count:5
Decomposition Temperature 300 - 350 °C572 - 662 °FAverage value: 306 °C Grade Count:16
UL RTI, Electrical 65.0 - 130 °C149 - 266 °FAverage value: 111 °C Grade Count:11
UL RTI, Mechanical with Impact 65.0 - 105 °C149 - 221 °FAverage value: 78.1 °C Grade Count:11
UL RTI, Mechanical without Impact 65.0 - 105 °C149 - 221 °FAverage value: 75.4 °C Grade Count:11
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:270
Flame Spread 30.0 mm/min1.18 in/minAverage value: 30.0 mm/min Grade Count:6
Oxygen Index 20.0 - 40.0 %20.0 - 40.0 %Average value: 24.7 % Grade Count:47
Glow Wire Test 649 - 960 °C1200 - 1760 °FAverage value: 790 °C Grade Count:46
Ignition Temperature 400 - 470 °C752 - 878 °FAverage value: 409 °C Grade Count:16
 
Processing PropertiesMetricEnglishComments
Processing Temperature 80.0 - 335 °C176 - 635 °FAverage value: 254 °C Grade Count:91
Nozzle Temperature 210 - 290 °C410 - 554 °FAverage value: 255 °C Grade Count:60
Die Temperature 215 - 245 °C419 - 473 °FAverage value: 235 °C Grade Count:6
Melt Temperature 200 - 330 °C392 - 626 °FAverage value: 256 °C Grade Count:348
Mold Temperature 10.0 - 140 °C50.0 - 284 °FAverage value: 71.5 °C Grade Count:355
Injection Velocity 50.0 - 60.0 mm/sec1.97 - 2.36 in/secAverage value: 55.0 mm/sec Grade Count:3
Drying Temperature 65.0 - 130 °C149 - 266 °FAverage value: 82.5 °C Grade Count:260
Moisture Content 0.000 - 2.00 %0.000 - 2.00 %Average value: 0.139 % Grade Count:145
Dew Point -40.0 - -17.8 °C-40.0 - 0.000 °FAverage value: -23.3 °C Grade Count:4
Injection Pressure 3.45 - 172 MPa500 - 25000 psiAverage value: 79.3 MPa Grade Count:36
Vent Depth 0.000762 cm0.000300 inAverage value: 0.000762 cm Grade Count:4
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 0.00350 %0.00350 %Average value: 0.00350 % Grade Count:3
TiO2 0.250 - 0.380 %0.250 - 0.380 %Average value: 0.277 % Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, Unreinforced
Overview of materials for Nylon 46, Unreinforced
Overview of materials for Nylon 66/6
Overview of materials for Nylon 6, 30% Glass Fiber Filled
Overview of materials for Polyetheretherketone, Unreinforced

O2400 / 77961

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.