MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Molybdenum Mo-0.5Ti; M0-0.5Ti-0.02C (Molybdenum Alloy 362)
Categories: Metal; Nonferrous Metal; Molybdenum Alloy; Refractory Metal

Key Words: UNS R03620, Specifications: ASTM B384, ASTM B385, ASTM B386, ASTM B387
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 10.2 g/cc0.368 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  76.0 MPa
@Temperature 1650 °C
11000 psi
@Temperature 3000 °F
 415 MPa
@Temperature 1095 °C
60200 psi
@Temperature 2003 °F
 895 MPa
@Temperature 23.0 °C
130000 psi
@Temperature 73.4 °F
Tensile Strength, Yield  48.0 MPa
@Temperature 1650 °C
6960 psi
@Temperature 3000 °F
 345 MPa
@Temperature 1095 °C
50000 psi
@Temperature 2003 °F
 825 MPa
@Temperature 23.0 °C
120000 psi
@Temperature 73.4 °F
Elongation at Break 10 %10 %
Tensile Modulus 315 GPa45700 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear 6.10 µm/m-°C
@Temperature 20.0 - 1010 °C
3.39 µin/in-°F
@Temperature 68.0 - 1850 °F
Specific Heat Capacity 0.250 J/g-°C0.0598 BTU/lb-°FEstimated from Pure Mo.
Thermal Conductivity 125 W/m-K868 BTU-in/hr-ft²-°FEstimated from Pure Mo.
Melting Point <= 2610 °C<= 4730 °F
Liquidus 2610 °C4730 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.010 - 0.040 %0.010 - 0.040 %
Iron, Fe <= 0.010 %<= 0.010 %
Molybdenum, Mo 99.5 %99.5 %
Nickel, Ni <= 0.0050 %<= 0.0050 %
Nitrogen, N <= 0.0010 %<= 0.0010 %
Oxygen, O <= 0.0030 %<= 0.0030 %
Silicon, Si <= 0.010 %<= 0.010 %
Titanium, Ti 0.40 - 0.55 %0.40 - 0.55 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Molybdenum, Mo, Annealed
Molybdenum TZC (Mo-1Ti-0.3Zr)
Overview of materials for Molybdenum Alloy
CuMoCu 13/74/13
W-50Mo Tungsten Alloy

MRMo00 / 13889

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.