MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Zirconium Copper (Amzirc Brand Copper), UNS C15000, TH04 Temper
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Excellent hot and cold workability. Fabricated by swaging, bending, heading, or forging.

Applications: Stud bases for power transmitters and rectifiers, switches and circuit breakers for high-temperature service, commutators, resistance welding tips and wheels, solderless wrapped connectors.

Mechanical property data for TH04 Temper - 82% cold work.

Key Words: ISO CuZr, CEN CW120C, N-4 Alloy
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.89 g/cc0.321 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 7272TB04 or TH04 temper
Tensile Strength, Ultimate  445 MPa
@Temperature 22.0 °C
64500 psi
@Temperature 71.6 °F
 463 MPa
@Temperature -78.0 °C
67200 psi
@Temperature -108 °F
 534 MPa
@Temperature -197 °C
77500 psi
@Temperature -323 °F
 587 MPa
@Temperature -253 °C
85100 psi
@Temperature -423 °F
 591 MPa
@Temperature -269 °C
85700 psi
@Temperature -452 °F
Tensile Strength, Yield 385 MPa55800 psi
 411 MPa
@Strain 0.2 %,
Temperature 22.0 °C
59600 psi
@Strain 0.2 %,
Temperature 71.6 °F
 423 MPa
@Strain 0.2 %,
Temperature -78.0 °C
61400 psi
@Strain 0.2 %,
Temperature -108 °F
 446 MPa
@Strain 0.2 %,
Temperature -269 °C
64700 psi
@Strain 0.2 %,
Temperature -452 °F
 453 MPa
@Strain 0.2 %,
Temperature -197 °C
65700 psi
@Strain 0.2 %,
Temperature -323 °F
 458 MPa
@Strain 0.2 %,
Temperature -253 °C
66400 psi
@Strain 0.2 %,
Temperature -423 °F
Elongation at Break  16 %
@Temperature 22.0 °C
16 %
@Temperature 71.6 °F
 20 %
@Temperature -78.0 °C
20 %
@Temperature -108 °F
 26 %
@Temperature -197 °C
26 %
@Temperature -323 °F
 36 %
@Temperature -269 °C
36 %
@Temperature -452 °F
 37 %
@Temperature -253 °C
37 %
@Temperature -423 °F
Creep Strength  1.00 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
145 psi
@Temperature 1200 °F,
Time 100000 hour
1% creep
 1.50 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
218 psi
@Temperature 1110 °F,
Time 100000 hour
1% creep
 1.70 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
247 psi
@Temperature 1200 °F,
Time 10000 hour
1% creep
 2.80 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
406 psi
@Temperature 1110 °F,
Time 10000 hour
1% creep
 3.00 MPa
@Temperature 650 °C,
Time 3.60e+6 sec
435 psi
@Temperature 1200 °F,
Time 1000 hour
1% creep
 5.20 MPa
@Temperature 600 °C,
Time 3.60e+6 sec
754 psi
@Temperature 1110 °F,
Time 1000 hour
1% creep
 28.0 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
4060 psi
@Temperature 932 °F,
Time 100000 hour
1% creep
 41.0 MPa
@Temperature 500 °C,
Time 3.60e+7 sec
5950 psi
@Temperature 932 °F,
Time 10000 hour
1% creep
 44.0 MPa
@Temperature 450 °C,
Time 3.60e+8 sec
6380 psi
@Temperature 842 °F,
Time 100000 hour
1% creep
 53.0 MPa
@Temperature 450 °C,
Time 3.60e+7 sec
7690 psi
@Temperature 842 °F,
Time 10000 hour
1% creep
 63.0 MPa
@Temperature 500 °C,
Time 3.60e+6 sec
9140 psi
@Temperature 932 °F,
Time 1000 hour
1% creep
 77.0 MPa
@Temperature 450 °C,
Time 3.60e+6 sec
11200 psi
@Temperature 842 °F,
Time 1000 hour
1% creep
 139 MPa
@Temperature 400 °C,
Time 3.60e+8 sec
20200 psi
@Temperature 752 °F,
Time 100000 hour
1% creep
 161 MPa
@Temperature 400 °C,
Time 3.60e+7 sec
23400 psi
@Temperature 752 °F,
Time 10000 hour
1% creep
 201 MPa
@Temperature 400 °C,
Time 3.60e+6 sec
29200 psi
@Temperature 752 °F,
Time 1000 hour
1% creep
 219 MPa
@Temperature 350 °C,
Time 3.60e+8 sec
31800 psi
@Temperature 662 °F,
Time 100000 hour
1% creep
 238 MPa
@Temperature 350 °C,
Time 3.60e+7 sec
34500 psi
@Temperature 662 °F,
Time 10000 hour
1% creep
 240 MPa
@Temperature 300 °C,
Time 3.60e+8 sec
34800 psi
@Temperature 572 °F,
Time 100000 hour
1% creep
 257 MPa
@Temperature 350 °C,
Time 3.60e+6 sec
37300 psi
@Temperature 662 °F,
Time 1000 hour
1% creep
 271 MPa
@Temperature 300 °C,
Time 3.60e+7 sec
39300 psi
@Temperature 572 °F,
Time 10000 hour
1% creep
 303 MPa
@Temperature 250 °C,
Time 3.60e+8 sec
43900 psi
@Temperature 482 °F,
Time 100000 hour
1% creep
 305 MPa
@Temperature 300 °C,
Time 3.60e+6 sec
44200 psi
@Temperature 572 °F,
Time 1000 hour
1% creep
 312 MPa
@Temperature 250 °C,
Time 3.60e+7 sec
45300 psi
@Temperature 482 °F,
Time 10000 hour
1% creep
 321 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
46600 psi
@Temperature 482 °F,
Time 1000 hour
1% creep
Modulus of Elasticity 129 GPa18700 ksi
Machinability 20 %20 %UNS C36000 (free-cutting brass) = 100%
Charpy Impact  121 J
@Temperature 22.0 °C
89.2 ft-lb
@Temperature 71.6 °F
V-notch, 10 mm square
 142 J
@Temperature -78.0 °C
105 ft-lb
@Temperature -108 °F
V-notch, 10 mm square
 155 J
@Temperature -197 °C
114 ft-lb
@Temperature -323 °F
V-notch, 10 mm square
 155 J
@Temperature -253 °C
114 ft-lb
@Temperature -423 °F
V-notch, 10 mm square
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000186 ohm-cm
@Temperature 20.0 °C
0.00000186 ohm-cm
@Temperature 68.0 °F
solution treated, cold worked 84%, and aged material
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.9 µm/m-°C
@Temperature 20.0 - 100 °C
9.39 µin/in-°F
@Temperature 68.0 - 212 °F
 17.6 µm/m-°C
@Temperature 20.0 - 200 °C
9.78 µin/in-°F
@Temperature 68.0 - 392 °F
 20.2 µm/m-°C
@Temperature 20.0 - 300 °C
11.2 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.385 J/g-°C0.0920 BTU/lb-°F
Thermal Conductivity 367 W/m-K2550 BTU-in/hr-ft²-°FSolution treated, cold worked 84%, and aged material
Melting Point 980 - 1080 °C1800 - 1980 °F
Solidus 980 °C1800 °F
Liquidus 1080 °C1980 °F
Annealing Point 899 - 949 °C1650 - 1740 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 600 - 700 °C1110 - 1290 °F
Hot-Working Temperature 900 - 950 °C1650 - 1740 °F
Precipitation Temperature >= 499 °C
@Time 7200 sec
>= 930 °F
@Time 2.00 hour
Water
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 99.9 %99.9 %
Zirconium, Zr 0.050 - 0.15 %0.050 - 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Zirconium Copper (Amzirc Brand Copper), UNS C15000, TH01 Temper
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, H04 Temper flat products
Zirconium Copper (Amzirc Brand Copper), UNS C15000, 19 mm rod
Oxygen-free extra-low phosphorus Copper, UNS C10300, H04 temper, flat products
Zirconium Copper (Amzirc Brand Copper), UNS C15000, 13 mm rod

MC15000d1 / 171639

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.