MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Overview of materials for Polyethylene Terephthalate (PET), 20% Glass Reinforced
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), 20% Glass Reinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyethylene Terephthalate (PET), 20% Glass Reinforced". Specific grades with glass content between 15% and 24% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.38 - 1.63 g/cc0.0499 - 0.0589 lb/in³Average value: 1.48 g/cc Grade Count:50
 1.17 - 1.17 g/cc
@Temperature 285 - 285 °C
0.0423 - 0.0423 lb/in³
@Temperature 545 - 545 °F
Average value: 1.17 g/cc Grade Count:1
Filler Content 15.0 - 20.0 %15.0 - 20.0 %Average value: 16.5 % Grade Count:10
Water Absorption 0.0500 - 2.50 %0.0500 - 2.50 %Average value: 0.394 % Grade Count:21
Moisture Absorption at Equilibrium 0.100 - 0.250 %0.100 - 0.250 %Average value: 0.208 % Grade Count:13
Viscosity  180000 - 180000 cP
@Temperature 280 - 280 °C
180000 - 180000 cP
@Temperature 536 - 536 °F
Average value: 180000 cP Grade Count:1
 180000 - 180000 cP
@Shear Rate 1000 - 1000 1/s
180000 - 180000 cP
@Shear Rate 1000 - 1000 1/s
Average value: 180000 cP Grade Count:1
Linear Mold Shrinkage 0.00100 - 0.0120 cm/cm0.00100 - 0.0120 in/inAverage value: 0.00438 cm/cm Grade Count:38
 0.00300 - 0.00300 cm/cm
@Temperature 275 - 275 °C
0.00300 - 0.00300 in/in
@Temperature 527 - 527 °F
Average value: 0.00300 cm/cm Grade Count:2
 0.00300 - 0.00300 cm/cm
@Pressure 60.0 - 60.0 MPa
0.00300 - 0.00300 in/in
@Pressure 8700 - 8700 psi
Average value: 0.00300 cm/cm Grade Count:2
Linear Mold Shrinkage, Transverse 0.00100 - 0.0120 cm/cm0.00100 - 0.0120 in/inAverage value: 0.00869 cm/cm Grade Count:15
 0.0110 - 0.0110 cm/cm
@Temperature 275 - 275 °C
0.0110 - 0.0110 in/in
@Temperature 527 - 527 °F
Average value: 0.0110 cm/cm Grade Count:2
 0.0110 - 0.0110 cm/cm
@Pressure 60.0 - 60.0 MPa
0.0110 - 0.0110 in/in
@Pressure 8700 - 8700 psi
Average value: 0.0110 cm/cm Grade Count:2
Ash 15.0 - 83.0 %15.0 - 83.0 %Average value: 37.7 % Grade Count:3
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 58.0 - 12358.0 - 123Average value: 95.8 Grade Count:5
Hardness, Rockwell R 110 - 120110 - 120Average value: 115 Grade Count:11
Tensile Strength, Ultimate 75.0 - 160 MPa10900 - 23200 psiAverage value: 105 MPa Grade Count:40
Tensile Strength, Yield 1.06 - 115 MPa154 - 16700 psiAverage value: 63.1 MPa Grade Count:10
Elongation at Break 1.50 - 6.00 %1.50 - 6.00 %Average value: 3.00 % Grade Count:44
Modulus of Elasticity 4.30 - 9.00 GPa624 - 1310 ksiAverage value: 6.83 GPa Grade Count:23
Flexural Yield Strength 6.89 - 230 MPa1000 - 33400 psiAverage value: 141 MPa Grade Count:33
Flexural Modulus 2.07 - 9.70 GPa300 - 1410 ksiAverage value: 5.81 GPa Grade Count:37
Compressive Yield Strength 90.0 - 138 MPa13100 - 20000 psiAverage value: 122 MPa Grade Count:3
Poissons Ratio 0.340 - 0.3600.340 - 0.360Average value: 0.356 Grade Count:5
Izod Impact, Notched 0.340 - 1.33 J/cm0.637 - 2.50 ft-lb/inAverage value: 0.704 J/cm Grade Count:24
Izod Impact, Unnotched 2.67 - 4.27 J/cm5.00 - 8.00 ft-lb/inAverage value: 3.42 J/cm Grade Count:5
Izod Impact, Notched (ISO) 4.50 - 13.0 kJ/m²2.14 - 6.19 ft-lb/in²Average value: 8.25 kJ/m² Grade Count:17
 5.00 - 8.00 kJ/m²
@Temperature -30.0 - -30.0 °C
2.38 - 3.81 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 6.43 kJ/m² Grade Count:8
Izod Impact, Unnotched (ISO) 25.0 - 35.0 kJ/m²
@Temperature -30.0 - -30.0 °C
11.9 - 16.7 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 30.0 kJ/m² Grade Count:2
Charpy Impact Unnotched 2.00 - 5.50 J/cm²9.52 - 26.2 ft-lb/in²Average value: 3.98 J/cm² Grade Count:9
 1.50 - 2.50 J/cm²
@Temperature -30.0 - 5.00 °C
7.14 - 11.9 ft-lb/in²
@Temperature -22.0 - 41.0 °F
Average value: 2.22 J/cm² Grade Count:6
Charpy Impact, Notched 0.450 - 1.10 J/cm²2.14 - 5.24 ft-lb/in²Average value: 0.780 J/cm² Grade Count:18
 0.660 - 0.800 J/cm²
@Temperature -30.0 - -30.0 °C
3.14 - 3.81 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 0.752 J/cm² Grade Count:5
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+13 - 1.00e+18 ohm-cm1.00e+13 - 1.00e+18 ohm-cmAverage value: 4.70e+16 ohm-cm Grade Count:29
Surface Resistance 1.00e+13 - 1.00e+15 ohm1.00e+13 - 1.00e+15 ohmAverage value: 2.16e+14 ohm Grade Count:14
Dielectric Constant 3.30 - 4.603.30 - 4.60Average value: 4.01 Grade Count:11
Dielectric Strength 16.1 - 38.0 kV/mm410 - 965 kV/inAverage value: 25.8 kV/mm Grade Count:21
Dissipation Factor 0.00300 - 0.06540.00300 - 0.0654Average value: 0.0280 Grade Count:6
Comparative Tracking Index 15.0 - 399 V15.0 - 399 VAverage value: 251 V Grade Count:16
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.6 - 98.0 µm/m-°C7.00 - 54.4 µin/in-°FAverage value: 42.2 µm/m-°C Grade Count:15
 109 - 109 µm/m-°C
@Temperature 55.0 - 160 °C
60.6 - 60.6 µin/in-°F
@Temperature 131 - 320 °F
Average value: 109 µm/m-°C Grade Count:2
CTE, linear, Transverse to Flow 40.0 - 120 µm/m-°C22.2 - 66.7 µin/in-°FAverage value: 80.6 µm/m-°C Grade Count:5
 32.0 - 32.0 µm/m-°C
@Temperature 55.0 - 160 °C
17.8 - 17.8 µin/in-°F
@Temperature 131 - 320 °F
Average value: 32.0 µm/m-°C Grade Count:2
Melting Point 225 - 260 °C437 - 500 °FAverage value: 247 °C Grade Count:26
Deflection Temperature at 0.46 MPa (66 psi) 220 - 250 °C428 - 482 °FAverage value: 238 °C Grade Count:22
Deflection Temperature at 1.8 MPa (264 psi) 180 - 242 °C356 - 468 °FAverage value: 209 °C Grade Count:45
Deflection Temperature at 8.0 MPa 70.0 - 80.0 °C158 - 176 °FAverage value: 75.0 °C Grade Count:3
Vicat Softening Point 205 - 255 °C401 - 491 °FAverage value: 227 °C Grade Count:6
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:40
Flame Spread 33.0 - 80.0 mm/min1.30 - 3.15 in/minAverage value: 57.3 mm/min Grade Count:4
Oxygen Index 19.0 - 24.0 %19.0 - 24.0 %Average value: 20.7 % Grade Count:3
Glow Wire Test 625 - 960 °C1160 - 1760 °FAverage value: 767 °C Grade Count:10
 
Processing PropertiesMetricEnglishComments
Processing Temperature 135 - 293 °C275 - 560 °FAverage value: 264 °C Grade Count:13
Nozzle Temperature 271 - 300 °C520 - 572 °FAverage value: 286 °C Grade Count:4
Melt Temperature 230 - 300 °C446 - 572 °FAverage value: 277 °C Grade Count:17
Mold Temperature 40.0 - 163 °C104 - 325 °FAverage value: 107 °C Grade Count:27
Drying Temperature 116 - 150 °C240 - 302 °FAverage value: 128 °C Grade Count:18
Moisture Content 0.0100 - 0.200 %0.0100 - 0.200 %Average value: 0.0673 % Grade Count:15
Injection Pressure 55.0 - 138 MPa7980 - 20000 psiAverage value: 86.0 MPa Grade Count:8

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyethylene Terephthalate (PET), Unreinforced
Overview of materials for Polyethylene Terephthalate (PET), 30% Glass Reinforced
Overview of materials for Polyethylene Terephthalate (PET), 50% Glass Reinforced
Overview of materials for Polyethylene Terephthalate (PET), Glass Fiber Filled, Flame Retardant
Overview of materials for Polyethylene Terephthalate (PET), 40% Glass Reinforced

O3312 / 78198

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.