MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

COI Ceramics Nextel™ A-N720 Oxide Ceramic Matrix Composite, Alumina
Categories: Ceramic; Ceramic Matrix Composite; Oxide; Aluminum Oxide

Material Notes: Description: Oxide ceramic matrix composites products are based upon sol-gel derived matrices and 3M Corporation's Nextel™ fiber products. These materials can be used up to 1200ºC (2200ºF) in air environments and are primarily used in both Aerospace and Gas Turbine applications.

Ceramic Matrix System: Water Based Sol-Gel Processing, Versatile Matrix Chemistry

Typical Applications for Oxide CMCs: Rotocraft Exhaust Systems, Advanced Thermal, Advanced Combustor

Highest Temperature & Creep Performance

Information from COI Ceramics, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.73 g/cc0.0986 lb/in³
Porosity 25 %25 %
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 169 MPa24500 psi
 141 MPa
@Treatment Temp. 1200 °C
20500 psi
@Treatment Temp. 2190 °F
 148 MPa
@Treatment Temp. 1090 °C
21500 psi
@Treatment Temp. 1990 °F
 159 MPa
@Treatment Temp. 982 °C
23100 psi
@Treatment Temp. 1800 °F
Tensile Stress at Strain  60.0 MPa
@Strain 0.1 %,
Temperature 1200 °C
8700 psi
@Strain 0.1 %,
Temperature 2190 °F
 70.3 MPa
@Strain 0.1 %,
Temperature 25.0 °C
10200 psi
@Strain 0.1 %,
Temperature 77.0 °F
 120 MPa
@Strain 0.2 %,
Temperature 1200 °C
17400 psi
@Strain 0.2 %,
Temperature 2190 °F
 125 MPa
@Strain 0.2 %,
Temperature 25.0 °C
18100 psi
@Strain 0.2 %,
Temperature 77.0 °F
 160 MPa
@Strain 0.3 %,
Temperature 25.0 °C
23200 psi
@Strain 0.3 %,
Temperature 77.0 °F
 160 MPa
@Strain 0.3 %,
Temperature 1200 °C
23200 psi
@Strain 0.3 %,
Temperature 2190 °F
Creep Strength  100 MPa
@Temperature 1200 °C,
Time >=360000 sec
14500 psi
@Temperature 2190 °F,
Time >=100 hour
 110 MPa
@Temperature 1200 °C,
Time 177000 sec
16000 psi
@Temperature 2190 °F,
Time 49.17 hour
 110 MPa
@Temperature 1200 °C,
Time 89890 sec
16000 psi
@Temperature 2190 °F,
Time 24.97 hour
 125 MPa
@Temperature 1200 °C,
Time 27700 sec
18100 psi
@Temperature 2190 °F,
Time 7.69 hour
 125 MPa
@Temperature 1200 °C,
Time 27100 sec
18100 psi
@Temperature 2190 °F,
Time 7.53 hour
 150 MPa
@Temperature 1200 °C,
Time 1010 sec
21800 psi
@Temperature 2190 °F,
Time 0.280 hour
 165 MPa
@Temperature 1200 °C,
Time 324 sec
23900 psi
@Temperature 2190 °F,
Time 0.0900 hour
Tensile Modulus 70.0 GPa10200 ksi
Fatigue Strength  150 MPa
@# of Cycles >=100000 ,
Temperature 1200 °C
21800 psi
@# of Cycles >=100000 ,
Temperature 2190 °F
 165 MPa
@# of Cycles >=100000 ,
Temperature 1200 °C
23900 psi
@# of Cycles >=100000 ,
Temperature 2190 °F
 170 MPa
@# of Cycles >=100000 ,
Temperature 1200 °C
24700 psi
@# of Cycles >=100000 ,
Temperature 2190 °F
 175 MPa
@# of Cycles 97798 ,
Temperature 1200 °C
25400 psi
@# of Cycles 97798 ,
Temperature 2190 °F
 175 MPa
@# of Cycles 27742 ,
Temperature 1200 °C
25400 psi
@# of Cycles 27742 ,
Temperature 2190 °F
Shear Strength 12.5 MPa1810 psiShort Beam
 
Thermal PropertiesMetricEnglishComments
CTE, linear 6.00 µm/m-°C3.33 µin/in-°F
Maximum Service Temperature, Air 1200 °C2190 °F
 
Descriptive Properties
Nominal Fiber Volume (%)45

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
COI Ceramics Nextel™ AS-N720 Oxide Ceramic Matrix Composite, Aluminosilicate
COI Ceramics Nextel™ AS-N312 Oxide Ceramic Matrix Composite, Aluminosilicate
COI Ceramics Nextel™ AS-N650 Oxide Ceramic Matrix Composite, Aluminosilicate
COI Ceramics Nextel™ AS-N610 Oxide Ceramic Matrix Composite, Aluminosilicate
Silicon Carbide, Reaction-Bonded, SiSiC

CCOIC003 / 122043

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.