MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI adhesives

SABIC LEXAN™ Copolymer HPH4504 Polycarbonate (PC) (Americas)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Gamma Radiation Resistant

Material Notes: High heat specialty polycarbonate. For medical devices and pharmaceutical applications. Healthcare management of change, biocompatible (ISO10993 of USP Class VI). EtO, steam, gamma and e-beam sterilizable.

Features: Care Compliance

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
 1.205 g/cc1.205 g/ccASTM D792
Density 1.19 g/cc0.0430 lb/in³ASTM D792
 1.20 g/cc0.0434 lb/in³ISO 1183
Water Absorption 0.16 %
@Time 86400 sec
0.16 %
@Time 24.0 hour
ASTM D570
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.350 %0.350 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.16 %0.16 %ISO 62-1
Viscosity  3.0 cP
@Load 1.20 kg,
Temperature 300 °C
3.0 cP
@Load 2.65 lb,
Temperature 572 °F
MVR cc/10 min; ISO 1133
 12 cP
@Load 2.16 kg,
Temperature 330 °C
12 cP
@Load 4.76 lb,
Temperature 626 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0070 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0070 - 0.0080 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 3.0 g/10 min
@Load 1.20 kg,
Temperature 300 °C
3.0 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 8585ASTM D785
Hardness, Rockwell R 122122ASTM D785
Tensile Strength at Break 65.0 MPa9430 psi50 mm/min; ISO 527
 71.0 MPa10300 psi50 mm/min; ASTM D638
Tensile Strength, Yield 65.0 MPa9430 psi50 mm/min; ASTM D638
 65.0 MPa9430 psi50 mm/min; ISO 527
Elongation at Break >= 50 %>= 50 %50 mm/min; ISO 527
 122 %122 %50 mm/min; ASTM D638
Elongation at Yield 7.0 %7.0 %50 mm/min; ASTM D638
 7.0 %7.0 %50 mm/min; ISO 527
Tensile Modulus 2.09 GPa303 ksi5 mm/min; ASTM D638
 2.26 GPa328 ksi1 mm/min; ISO 527
Flexural Strength 66.0 MPa9570 psiyield, 2 mm/min; ISO 178
 95.0 MPa13800 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.02 GPa293 ksi1.3 mm/min, 50 mm span; ASTM D790
 2.12 GPa307 ksi2 mm/min; ISO 178
Izod Impact Notched 640 J472 ft-lbASTM D256
 144 J
@Temperature -30.0 °C
106 ft-lb
@Temperature -22.0 °F
ASTM D256
Izod Impact, Unnotched 32.04 J/cm60.02 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 13.0 kJ/m²6.19 ft-lb/in²80*10*4; ISO 180/1A
 11.0 kJ/m²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 1.50 J/cm²7.14 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Tensile Impact Strength 577 kJ/m²275 ft-lb/in²ASTM D1822
Dart Drop, Total Energy 73.0 J53.8 ft-lbASTM D3763
 149 J110 ft-lbASTM D3029
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 2.60e+17 ohm-cm>= 2.60e+17 ohm-cmASTM D257
Dielectric Constant  3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
ASTM D150
 3.15
@Frequency 50.0 - 60.0 Hz
3.15
@Frequency 50.0 - 60.0 Hz
ASTM D150
Dielectric Strength 20.3 kV/mm
@Thickness 3.20 mm
516 kV/in
@Thickness 0.126 in
in air; ASTM D149
Dissipation Factor  0.0012
@Frequency 50.0 - 60.0 Hz
0.0012
@Frequency 50.0 - 60.0 Hz
ASTM D150
 0.024
@Frequency 100 Hz
0.024
@Frequency 100 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
33.3 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 91.8 µm/m-°C
@Temperature -40.0 - 95.0 °C
51.0 µin/in-°F
@Temperature -40.0 - 203 °F
ASTM E831
CTE, linear, Transverse to Flow  60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
33.3 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
33.3 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Specific Heat Capacity 1.26 J/g-°C0.301 BTU/lb-°FASTM C351
Thermal Conductivity 0.210 W/m-K1.46 BTU-in/hr-ft²-°FASTM C177
Deflection Temperature at 1.8 MPa (264 psi) 132 °C270 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 143 °C
@Thickness 3.20 mm
289 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 154 °C309 °FRate B/50; ISO 306
 155 °C311 °FRate B/120; ISO 306
 160 °C320 °FRate B/50; ASTM D1525
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.601.60ASTM D542
Haze 1.0 %
@Thickness 2.54 mm
1.0 %
@Thickness 0.100 in
ASTM D1003
Transmission, Visible 85 %
@Thickness 2.54 mm
85 %
@Thickness 0.100 in
ASTM D1003
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 330 - 355 °C626 - 671 °F
Zone 2 325 - 350 °C617 - 662 °F
Zone 3 340 - 360 °C644 - 680 °F
Melt Temperature 340 - 360 °C644 - 680 °FInjection Molding
Mold Temperature 80.0 - 115 °C176 - 239 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 48.0 hour48.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 60 %40 - 60 %
Vent Depth 0.00250 - 0.00760 cm0.000984 - 0.00299 in
Screw Speed 40 - 70 rpm40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80357 / 288304

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.