MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Braskem H 216 HOMO Polypropylene Homopolymer  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Fiber Grade

Material Notes: H 216 is a high melt flow rate homopolymer with narrow molecular weight distribution. It is designed for fiber extrusion processing with high toughness fibers. H 216 exhibits excellent processability with good melt stability and toughness/impact balance. Its applications include: staple fibers and continuous filaments with high toughness and low denier; and fibers for reinforcement of asbestos-free concrete and roof tiles.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.905 g/cc0.0327 lb/in³ASTM-D792
Melt Flow 18 g/10 min
@Load 2.16 kg,
Temperature 230 °C
18 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM-D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 103103ASTM-D785
Tensile Strength, Yield 36.0 MPa5220 psiASTM-D638
Elongation at Yield 9.0 %9.0 %ASTM-D638
Flexural Modulus, 1% Secant 1400 MPa203000 psiASTM-D790
Izod Impact, Notched 0.250 J/cm0.468 ft-lb/inASTM-D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 103 °C217 °FASTM-D648
Deflection Temperature at 1.8 MPa (264 psi) 59.0 °C138 °FASTM-D648
Vicat Softening Point 151 °C
@Load 1.02 kg
304 °F
@Load 2.25 lb
ASTM-D1525

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Braskem H 503HS HOMO Polypropylene Homopolymer
Braskem H 214 HOMO Polypropylene Homopolymer
Braskem H 125 HOMO Polypropylene Homopolymer
Braskem PH 1721 HOMO Polypropylene Homopolymer
Braskem 6D43 Polypropylene Random Copolymer

PBRAS935 / 106781

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.