MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Mid-Mountain Materials CERMEX® PR1000-C Commercial Grade Thermal Insulation Paper
Categories: Ceramic; Glass; Glass Fiber; Other Engineering Material; Composite Fibers

Material Notes: Material: Non-respirable E-glass fibers
Construction: Felted paper, organic binder

Information provided by Mid-Mountain Materials

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density  0.111 g/cc
@Thickness 3.17 mm
0.00399 lb/in³
@Thickness 0.125 in
 0.112 g/cc
@Thickness 6.35 mm
0.00405 lb/in³
@Thickness 0.250 in
 0.176 g/cc
@Thickness 1.59 mm
0.00637 lb/in³
@Thickness 0.0625 in
Loss On Ignition 5.0 - 7.0 %5.0 - 7.0 %
Thickness 1587 microns62.48 mil
 3175 microns125.0 mil
 6360 microns250 mil
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  0.0350 W/m-K
@Temperature 24.0 °C
0.243 BTU-in/hr-ft²-°F
@Temperature 75.2 °F
N2; ASTM C177
 0.0450 W/m-K
@Temperature 100 °C
0.312 BTU-in/hr-ft²-°F
@Temperature 212 °F
N2; ASTM C177
 0.0600 W/m-K
@Temperature 200 °C
0.416 BTU-in/hr-ft²-°F
@Temperature 392 °F
N2; ASTM C177
 0.0600 W/m-K
@Temperature 200 °C
0.416 BTU-in/hr-ft²-°F
@Temperature 392 °F
Air; ASTM C114
 0.0810 W/m-K
@Temperature 300 °C
0.562 BTU-in/hr-ft²-°F
@Temperature 572 °F
Air; ASTM C114
 0.105 W/m-K
@Temperature 400 °C
0.729 BTU-in/hr-ft²-°F
@Temperature 752 °F
Air; ASTM C114
Melting Point >= 1100 °C>= 2010 °FFiber Only
Maximum Service Temperature, Air 538 °C1000 °FContinuous
 649 °C1200 °FIntermittent
 
Descriptive Properties
ColorWhite
Tensile Strength (lbs/in)221/16", Cross Direction
 251/16", Machine Direction
 331/8", Machine Direction
 341/8", Cross Direction
 69.21/4", Machine Direction
 81.71/4", Cross Direction
Width (in)51Standard

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chosun Refractories 1260PAPER Paper
Chosun Refractories 1500 ACE PAPER Paper
ITW Insulation TRYMER® 1800 Polyisocyanurate Insulation
Thermal Ceramics BTU-GUE
3M 4317 Single-Coated Foam Tape

CMID66 / 141234

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.