  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Norplex-Micarta EnableX™ 10 oz WR - 30% Vinyl Ester Prepreg System
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Vinyl Ester

Material Notes: EnableX™ allows continuous fiber pre-preg to be co-cured in a multi-material molding system to produce near net shapes. Building upon the predictability of continuous fiber reinforced pre-preg, EnableX™ materials are ppecifically designed for compression molding and tested to ensure compatibility. The in-house laboratory and development capabilities allow for new concepts to be prototyped, or specific datasets to be developed to support specific design criteria.

Features:

  • Superior specific strength and stiffness
  • Inherent chemical resistance
  • Excellent dielectric properties
  • Self-lubricating and low wear
  • Low FST generation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.09 g/cc2.09 g/ccASTM D792
Moisture Absorption 0.0700 %0.0700 %Condition A; ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 101101ASTM D785
Tensile Strength 282 MPa40900 psiCondition A, CW; ASTM D3039
 405 MPa58700 psiCondition A, LW; ASTM D3039
 169 MPa
@Temperature 155 °C
24500 psi
@Temperature 311 °F
LW; ASTM D3039
 248 MPa
@Temperature 155 °C
35900 psi
@Temperature 311 °F
CW; ASTM D3039
Tensile Modulus 22.4 GPa3250 ksiCondition A, CW; ASTM D3039
 28.6 GPa4150 ksiCondition A, LW; ASTM D3039
 25.9 GPa
@Temperature 155 °C
3750 ksi
@Temperature 311 °F
CW; ASTM D3039
 34.1 GPa
@Temperature 155 °C
4940 ksi
@Temperature 311 °F
LW; ASTM D3039
Flexural Strength  107 MPa
@Temperature 175 °C
15500 psi
@Temperature 347 °F
CW; ASTM D790
 139 MPa
@Temperature 175 °C
20100 psi
@Temperature 347 °F
LW; ASTM D790
 149 MPa
@Temperature 155 °C
21600 psi
@Temperature 311 °F
CW; ASTM D790
 174 MPa
@Temperature 135 °C
25200 psi
@Temperature 275 °F
CW; ASTM D790
 181 MPa
@Temperature 155 °C
26300 psi
@Temperature 311 °F
LW; ASTM D790
 192 MPa
@Temperature 135 °C
27800 psi
@Temperature 275 °F
LW; ASTM D790
 205 MPa
@Temperature 120 °C
29700 psi
@Temperature 248 °F
CW; ASTM D790
 245 MPa
@Temperature 120 °C
35500 psi
@Temperature 248 °F
LW; ASTM D790
 271 MPa
@Temperature 23.0 °C
39300 psi
@Temperature 73.4 °F
Condition A, CW; ASTM D790
 348 MPa
@Temperature 23.0 °C
50500 psi
@Temperature 73.4 °F
Condition A, LW; ASTM D790
Flexural Modulus  19.9 GPa
@Temperature 175 °C
2880 ksi
@Temperature 347 °F
CW; ASTM D790
 20.7 GPa
@Temperature 175 °C
3000 ksi
@Temperature 347 °F
LW; ASTM D790
 20.8 GPa
@Temperature 155 °C
3010 ksi
@Temperature 311 °F
CW; ASTM D790
 21.5 GPa
@Temperature 155 °C
3120 ksi
@Temperature 311 °F
LW; ASTM D790
 24.0 GPa
@Temperature 135 °C
3480 ksi
@Temperature 275 °F
CW; ASTM D790
 25.3 GPa
@Temperature 120 °C
3670 ksi
@Temperature 248 °F
CW; ASTM D790
 25.9 GPa
@Temperature 135 °C
3760 ksi
@Temperature 275 °F
LW; ASTM D790
 26.5 GPa
@Temperature 120 °C
3840 ksi
@Temperature 248 °F
LW; ASTM D790
 27.0 GPa
@Temperature 23.0 °C
3910 ksi
@Temperature 73.4 °F
Condition A, CW; ASTM D790
 28.1 GPa
@Temperature 23.0 °C
4080 ksi
@Temperature 73.4 °F
Condition A, LW; ASTM D790
Compressive Strength  473 MPa
@Temperature 155 °C
68600 psi
@Temperature 311 °F
ASTM D695
 667 MPa
@Temperature 23.0 °C
96700 psi
@Temperature 73.4 °F
Condition A; ASTM D695
Compressive Modulus  4.62 GPa
@Temperature 155 °C
670 ksi
@Temperature 311 °F
ASTM D695
 6.48 GPa
@Temperature 23.0 °C
940 ksi
@Temperature 73.4 °F
Condition A; ASTM D695
Shear Strength 22.8 MPa3300 psiCondition A, Short Beam, CW; ASTM D3518
 22.8 MPa3300 psiCondition A, Short Beam, LW; ASTM D2344
Izod Impact, Unnotched 20.0 J/cm37.5 ft-lb/inCW; ASTM D256
 22.2 J/cm41.5 ft-lb/inLW; ASTM D256
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 130 °C266 °FCondition A, TMA; ASTM D7028
Flammability, UL94 V-1V-1Condition A

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PNORPM266 / 280540

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.