MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type A7 Tool Steel
Categories: Metal; Ferrous Metal; Tool Steel; Air-Hardening Steel; Cold Work Steel

Material Notes: High hardenability, high degree of dimensional stability in heat treatment, good wear resistance, fatigue life, toughness, and deep hardening qualities. Applications include cold forming, blanking and bending dies, forming rolls, drill bushings, knurling tools, master dies and gauges.

Key Words: AISI Medium-Alloy, Air-Hardening Tool Steels A7, UNS T30107, ASTM A681, FED QQ-T-570
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.66 g/cc0.277 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 58 - 6658 - 66
 65 - 66.565 - 66.5as air quenched from 955°C
 44 - 46
@Tempering Temp. 650 °C,
Time 10800 sec
44 - 46
@Tempering Temp. 1200 °F,
Time 3.00 hour
air quenched from 955°C then tempered for 3 hours
 53 - 55
@Tempering Temp. 595 °C,
Time 10800 sec
53 - 55
@Tempering Temp. 1100 °F,
Time 3.00 hour
air quenched from 955°C then tempered for 3 hours
 56 - 58
@Tempering Temp. 540 °C,
Time 10800 sec
56 - 58
@Tempering Temp. 1000 °F,
Time 3.00 hour
air quenched from 955°C then tempered for 3 hours
 59 - 61
@Tempering Temp. 425 °C,
Time 10800 sec
59 - 61
@Tempering Temp. 797 °F,
Time 3.00 hour
air quenched from 955°C then tempered for 3 hours
 61 - 63
@Tempering Temp. 315 °C,
Time 10800 sec
61 - 63
@Tempering Temp. 599 °F,
Time 3.00 hour
air quenched from 955°C then tempered for 3 hours
 62 - 64
@Tempering Temp. 260 °C,
Time 10800 sec
62 - 64
@Tempering Temp. 500 °F,
Time 3.00 hour
air quenched from 955°C then tempered for 3 hours
 64 - 65
@Tempering Temp. 150 °C,
Time 10800 sec
64 - 65
@Tempering Temp. 302 °F,
Time 3.00 hour
air quenched from 955°C then tempered for 3 hours
Bulk Modulus 160 GPa23200 ksiTypical for steels.
Machinability 65 %65 %Based on Carbon tool steel.
Shear Modulus 80.0 GPa11600 ksiTypical for steels.
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C6.67 µin/in-°F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 150 - 540 °C302 - 1000 °FTempering Temperature
 955 - 980 °C1750 - 1800 °FHardening Temperature
Annealing Temperature 870 - 900 °C1600 - 1650 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 2.0 - 2.85 %2.0 - 2.85 %
Chromium, Cr 5.38 %5.38 %
Iron, Fe 84 %84 %As Balance
Manganese, Mn <= 0.80 %<= 0.80 %
Molybdenum, Mo 1.15 %1.15 %
Phosphorus, P <= 0.030 %<= 0.030 %
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.030 %<= 0.030 %
Tungsten, W 1 %1 %Optional
Vanadium, V 4.53 %4.53 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type A2 Tool Steel
AISI Type A6 Tool Steel
AISI Type A4 Tool Steel
AISI Type A10 Tool Steel
AISI Type O6 Tool Steel

MSTA7A / 14100

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.