MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Medium Density Polyethylene (MDPE), Film Grade
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Medium Density (MDPE); Medium Density Polyethylene (MDPE), Film Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Medium Density Polyethylene (MDPE), Film Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.925 - 0.958 g/cc0.0334 - 0.0346 lb/in³Average value: 0.937 g/cc Grade Count:32
Water Vapor Transmission 7.76 - 14.0 g/m²/day0.500 - 0.900 g/100 in²/dayAverage value: 11.4 g/m²/day Grade Count:4
 10.864 - 12.416 g/m²/day
@Temperature 37.8 - 37.8 °C
0.69964 - 0.79959 g/100 in²/day
@Temperature 100 - 100 °F
Average value: 11.6 g/m²/day Grade Count:2
Oxidative Induction Time (OIT) 25.0 - 30.0 min
@Temperature 200 - 200 °C
25.0 - 30.0 min
@Temperature 392 - 392 °F
Average value: 27.0 min Grade Count:6
Thickness 20.0 - 38.1 microns0.787 - 1.50 milAverage value: 27.5 microns Grade Count:12
Melt Flow 0.0570 - 30.0 g/10 min0.0570 - 30.0 g/10 minAverage value: 6.77 g/10 min Grade Count:32
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 60.060.0Average value: 60.0 Grade Count:6
Film Tensile Strength at Yield, MD 12.4 - 35.2 MPa1800 - 5100 psiAverage value: 20.7 MPa Grade Count:23
Film Tensile Strength at Yield, TD 14.7 - 29.6 MPa2130 - 4300 psiAverage value: 19.6 MPa Grade Count:23
Tensile Strength, Yield 18.0 - 27.6 MPa2610 - 4000 psiAverage value: 21.9 MPa Grade Count:3
Film Elongation at Break, MD 150 - 800 %150 - 800 %Average value: 529 % Grade Count:29
Film Elongation at Break, TD 10.0 - 900 %10.0 - 900 %Average value: 666 % Grade Count:29
Elongation at Break 600 - 910 %600 - 910 %Average value: 797 % Grade Count:3
Flexural Modulus 0.590 - 0.850 GPa85.6 - 123 ksiAverage value: 0.751 GPa Grade Count:13
Secant Modulus, MD 0.214 - 1.07 GPa31.0 - 155 ksiAverage value: 0.431 GPa Grade Count:15
Secant Modulus, TD 0.172 - 1.37 GPa25.0 - 199 ksiAverage value: 0.514 GPa Grade Count:15
Izod Impact, Notched 1.15 - 8.00 J/cm2.15 - 15.0 ft-lb/inAverage value: 4.92 J/cm Grade Count:3
Elmendorf Tear Strength MD 10.0 - 350 g10.0 - 350 gAverage value: 72.7 g Grade Count:20
Elmendorf Tear Strength TD 35.0 - 1450 g35.0 - 1450 gAverage value: 508 g Grade Count:20
Elmendorf Tear Strength, MD 0.800 - 3.94 g/micron20.3 - 100 g/milAverage value: 1.83 g/micron Grade Count:9
Elmendorf Tear Strength, TD 3.94 - 19.7 g/micron100 - 500 g/milAverage value: 13.7 g/micron Grade Count:9
Dart Drop 1.57 - 5.91 g/micron40.0 - 150 g/milAverage value: 3.39 g/micron Grade Count:8
Dart Drop Test 30.0 - 300 g0.0662 - 0.662 lbAverage value: 110 g Grade Count:26
Film Tensile Strength at Break, MD 4.83 - 76.5 MPa700 - 11100 psiAverage value: 47.1 MPa Grade Count:29
Film Tensile Strength at Break, TD 17.0 - 66.2 MPa2470 - 9600 psiAverage value: 38.9 MPa Grade Count:29
 
Thermal PropertiesMetricEnglishComments
Melting Point 116 - 272 °C241 - 522 °FAverage value: 133 °C Grade Count:16
Vicat Softening Point 116 - 124 °C241 - 255 °FAverage value: 120 °C Grade Count:12
 
Optical PropertiesMetricEnglishComments
Haze 4.80 - 52.0 %4.80 - 52.0 %Average value: 11.6 % Grade Count:12
Gloss 12.0 - 90.0 %12.0 - 90.0 %Average value: 60.1 % Grade Count:13
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 220 °C68.0 - 428 °FAverage value: 188 °C Grade Count:11
Melt Temperature 193 - 280 °C380 - 536 °FAverage value: 219 °C Grade Count:5

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Low Density Polyethylene (LDPE), Film Grade
Overview of materials for High Density Polyethylene (HDPE), Film Grade
Overview of materials for Medium Density Polyethylene (MDPE), Molded
Overview of materials for Low Density Polyethylene (LDPE), Molded
Overview of materials for Linear Low Density Polyethylene (LLDPE), Film Grade

O3907 / 78271

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.