MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Bada BADALAC® UL ABS 30 FR01 natural
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Unreinforced, Flame Retardant

Material Notes: Easy-flowing ABS injection molding grade; halogenated and flame-protected; convenient for colors

Information provided by Bada

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.23 g/cc0.0444 lb/in³ISO 1183
Moisture Absorption 0.240 %0.240 %50% r.h.; ISO 62
Water Absorption at Saturation 0.95 %0.95 %ISO 62
Melt Flow 10 g/10 min
@Load 10.0 kg,
Temperature 220 °C
10 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 38.0 MPa5510 psi50 mm/min; ISO 527-1/2
Elongation at Yield 2.5 %2.5 %50 mm/min; ISO 527-1/2
Tensile Modulus 2.40 GPa348 ksi1 mm/min; ISO 527-1/2
Charpy Impact Unnotched 3.50 J/cm²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.700 J/cm²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC-62631-3-1
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC-62631-3-1
Dielectric Constant 2.8
@Frequency 1e+6 Hz
2.8
@Frequency 1e+6 Hz
IEC-62631-2-1
Dielectric Strength 38.0 kV/mm965 kV/inIEC-60243-1
Dissipation Factor 0.079
@Frequency 1e+6 Hz
0.079
@Frequency 1e+6 Hz
IEC-62631-2-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 80.0 - 110 µm/m-°C44.4 - 61.1 µin/in-°FISO 11359-2
Maximum Service Temperature, Air 90.0 °C194 °Fsome hours; EC-60216
Deflection Temperature at 0.46 MPa (66 psi) 99.0 °C210 °FISO 75-1/2
Deflection Temperature at 1.8 MPa (264 psi) 94.0 °C201 °FISO 75-1/2
Vicat Softening Point 95.0 °C203 °FVST B50; ISO 306
 102 °C216 °FVST A50; ISO 306
Flammability, UL94  V-0
@Thickness 0.750 mm
V-0
@Thickness 0.0295 in
 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
 5VA
@Thickness 3.00 mm
5VA
@Thickness 0.118 in
Glow Wire Ignition Temperature 700 °C
@Thickness 1.50 mm
1290 °F
@Thickness 0.0591 in
IEC-60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 1.50 mm
1760 °F
@Thickness 0.0591 in
IEC-60695-2-12
 
Processing PropertiesMetricEnglishComments
Melt Temperature 220 - 260 °C428 - 500 °F
Mold Temperature 30.0 - 80.0 °C86.0 - 176 °F
Drying Temperature 80.0 °C176 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Moisture Content <= 0.10 %<= 0.10 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBADA389 / 287222

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.