MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Ascend Performance Materials HiDura™ D1MG33J BK0816 Nylon 612, 33% Glass Fiber Reinforced, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 612 (PA612); Nylon 612, Glass Fiber Filler

Material Notes: Product Description: HiDura D1MG33J BK0816 is an organically heat stabilized, 33% glass filled PA612 designed for injection molding applications.

Availability: Asia Pacific; Europe; North America

Features: Chemical Resistant; Good Thermal Stability; Heat Stabilized – Organic

Uses: Automotive Applications; Connectors

Appearance: Black

Forms: Pellets

Processing Method: Injection Molding

Information provided by Ascend Performance Materials Operations LLC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.32 g/cc0.0477 lb/in³ISO 1183
Water Absorption 0.80 %0.80 %Equilibrium, 50% RH; ISO 62
 0.30 %
@Time 86400 sec
0.30 %
@Time 24.0 hour
ISO 62
Linear Mold Shrinkage, Flow 0.013 cm/cm
@Thickness 2.00 mm
0.013 in/in
@Thickness 0.0787 in
ISO 294-4
Linear Mold Shrinkage, Transverse 0.0040 cm/cm
@Thickness 2.00 mm
0.0040 in/in
@Thickness 0.0787 in
ISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 127 MPa18400 psiISO 527-2
Elongation at Break 5.0 %5.0 %ISO 527-2
Tensile Modulus 7.93 GPa1150 ksiISO 527-2
Flexural Strength 177 MPa25700 psiISO 178
Flexural Modulus 7.79 GPa1130 ksiISO 178
Izod Impact, Notched (ISO)  9.24 kJ/m²
@Temperature -40.0 °C
4.40 ft-lb/in²
@Temperature -40.0 °F
ISO 180
 9.87 kJ/m²
@Temperature -30.0 °C
4.70 ft-lb/in²
@Temperature -22.0 °F
ISO 180
 13.0 kJ/m²
@Temperature 22.8 °C
6.20 ft-lb/in²
@Temperature 73.0 °F
ISO 180
Charpy Impact Unnotched  6.51 J/cm²
@Temperature -40.0 °C
31.0 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eU
 6.93 J/cm²
@Temperature -30.0 °C
33.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 7.77 J/cm²
@Temperature 22.8 °C
37.0 ft-lb/in²
@Temperature 73.0 °F
ISO 179/1eU
Charpy Impact, Notched  1.01 J/cm²
@Temperature -40.0 °C
4.80 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eA
 1.01 J/cm²
@Temperature -30.0 °C
4.80 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 1.41 J/cm²
@Temperature 22.8 °C
6.70 ft-lb/in²
@Temperature 73.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 31.1 kV/mm790 kV/inIEC 60243
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 210 °C410 °FUnannealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 191 °C376 °FUnannealed; ISO 75-2/A
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 - 300 °C464 - 572 °F
Mold Temperature 60.0 - 120 °C140 - 248 °F
Drying Temperature 80.0 °C176 °F
Dry Time <= 4.00 hour<= 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PASCF1029 / 310722

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.