MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Alclad Aluminum 2024-T72
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Key Words: UNS A82024
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.77 g/cc0.100 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  >= 385 MPa
@Thickness 0.254 - 1.57 mm
>= 55800 psi
@Thickness 0.0100 - 0.0620 in
Sheet
 >= 400 MPa
@Thickness 1.60 - 6.32 mm
>= 58000 psi
@Thickness 0.0630 - 0.249 in
Sheet
Tensile Strength, Yield  >= 295 MPa
@Thickness 0.254 - 1.57 mm
>= 42800 psi
@Thickness 0.0100 - 0.0620 in
Sheet
 >= 310 MPa
@Thickness 1.60 - 6.32 mm
>= 45000 psi
@Thickness 0.0630 - 0.249 in
Sheet
Elongation at Break  >= 5.0 %
@Thickness 0.254 - 1.57 mm
>= 5.0 %
@Thickness 0.0100 - 0.0620 in
Sheet
 >= 5.0 %
@Thickness 1.60 - 6.32 mm
>= 5.0 %
@Thickness 0.0630 - 0.249 in
Sheet
Modulus of Elasticity 72.4 GPa10500 ksi
Poissons Ratio <= 0.33<= 0.33
Shear Modulus 28.0 GPa4060 ksi
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.1 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.7 µin/in-°F
@Temperature -58.0 - 68.0 °F
 22.9 µm/m-°C
@Temperature 20.0 - 100 °C
12.7 µin/in-°F
@Temperature 68.0 - 212 °F
 23.8 µm/m-°C
@Temperature 20.0 - 200 °C
13.2 µin/in-°F
@Temperature 68.0 - 392 °F
 24.7 µm/m-°C
@Temperature 20.0 - 300 °C
13.7 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.875 J/g-°C0.209 BTU/lb-°F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al >= 99.3 %>= 99.3 %
Copper, Cu <= 0.10 %<= 0.10 %
Magnesium, Mg <= 0.050 %<= 0.050 %
Manganese, Mn <= 0.050 %<= 0.050 %
Other, each <= 0.030 %<= 0.030 %
Si+Fe <= 0.70 %<= 0.70 %
Titanium, Ti <= 0.030 %<= 0.030 %
Vanadium, V <= 0.050 %<= 0.050 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Alclad Aluminum 2024-T62
Alclad Aluminum 2024-T42
Alclad Aluminum 2024-T81, T851
Alclad Aluminum 2024-T861
Aluminum 2024-T6

MA2024AT72 / 109167

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.