MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Akro-Plastic Akrotek® PEEK TM black (5051) PEEK, Dry
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Unreinforced

Material Notes: Description: AKROTEK® PEEK TM black (5051) is an unreinforced polyetheretherketone with good tribological properties

Applications: Applications are mainly elements in the automotive-, aeronautical-, industrial- and medical engineering that require low friction and wear values in a temperature environment above 150 °C

Information provided by Akro-Plastic GmbH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.46 g/cc0.0527 lb/in³ISO 1183
 
Mechanical PropertiesMetricEnglishComments
Elongation at Break 2.2 %2.2 %50 [mm/min]; ISO 527-2
Tensile Modulus 6.00 GPa870 ksi1 [mm/min]; ISO 527-2
Flexural Strength 135 MPa19600 psi2 [mm/min]; ISO 178
Flexural Modulus 6.00 GPa870 ksi2 [mm/min]; ISO 178
Flexural Strain at Break 4.0 %4.0 %2 mm/min; ISO 178
Charpy Impact Unnotched 3.50 J/cm²
@Temperature 23.0 °C
16.7 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 0.300 J/cm²
@Temperature 23.0 °C
1.43 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 342 °C648 °FDSC, 10K/min; DIN EN 11357-1
Deflection Temperature at 8.0 MPa 145 °C293 °FISO 75/C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyetheretherketone, Unreinforced
Akro-Plastic Akrotek® PEEK natural (5184) PEEK, Dry
Overview of materials for Polyetheretherketone, Glass Fiber Filled
Akro-Plastic Akrotek® PEEK CF 30 black (5049) PEEK, Conditioned, 30% Carbon Filled
Akro-Plastic Akrotek® PEEK GF 50 natural (5100) PEEK, Conditioned, 50% Glass Filled

PAKRO444 / 183031

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.