MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

CMW® 3 Copper Alloy  (discontinued **)
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: CMW® 3 material is a high strength, high conductivity copper base alloy. CMW® 3 material is heat treatable. Optimum mechanical and physical properties of CMW® 3 material are developed by heat treatment or through a combination of heat treatment and cold working.

CMW® 3 material is used extensively for spot welding electrodes and is well suited for custom bent designs, flash welding dies, and seam welding wheels, and provides better performance and greater savings than other copper alloys used for spot and seam welding.

Property data for fully precipitation heat treated condition.

Information provided by CMW Inc.

1

Key Words: UNS C18200 (Wrought); UNS C18500 (Cast)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.89 g/cc0.321 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 6868Forging (Hot Forged and Heat Treated)
 6868Premium Casting
 7878Premium Forging (Hot Forged, Heat Treated, and Cold Worked to less than 1" thick)
 8080Strip (TH04)
 75
@Thickness <=25.0 mm
75
@Thickness <=0.984 in
Plate
 83
@Diameter <=25.0 mm
83
@Diameter <=0.984 in
Drawn Rod & Bar
Tensile Strength, Ultimate 345 MPa50000 psiPremium Casting
 414 MPa60000 psiForging (Hot Forged and Heat Treated)
 469 MPa68000 psiPremium Forging (Hot Forged, Heat Treated, and Cold Worked to less than 1" thick)
 517 MPa75000 psiStrip (TH04)
 448 MPa
@Thickness <=25.0 mm
65000 psi
@Thickness <=0.984 in
Plate
 517 MPa
@Diameter <=25.0 mm
75000 psi
@Diameter <=0.984 in
Drawn Rod & Bar
Tensile Strength, Yield 276 MPa40000 psiPremium Casting
 298 MPa43200 psiForging (Hot Forged and Heat Treated)
 414 MPa60000 psiPremium Forging (Hot Forged, Heat Treated, and Cold Worked to less than 1" thick)
 482 MPa69900 psiStrip (TH04)
 379 MPa
@Thickness <=25.0 mm
55000 psi
@Thickness <=0.984 in
Plate
 482 MPa
@Diameter <=25.0 mm
69900 psi
@Diameter <=0.984 in
Drawn Rod & Bar
Elongation at Break 3.0 %3.0 %Strip (TH04)
 17 %17 %Premium Forging (Hot Forged, Heat Treated, and Cold Worked to less than 1" thick)
 20 %20 %Premium Casting
 28 %28 %Forging (Hot Forged and Heat Treated)
 20 %
@Thickness <=25.0 mm
20 %
@Thickness <=0.984 in
Plate
 15 %
@Diameter <=25.0 mm
15 %
@Diameter <=0.984 in
Drawn Rod & Bar
Reduction of Area 45 %45 %Premium Casting
 65 %65 %Premium Forging (Hot Forged, Heat Treated, and Cold Worked to less than 1" thick)
 73 %73 %Forging (Hot Forged and Heat Treated)
 60 %
@Diameter <=25.0 mm
60 %
@Diameter <=0.984 in
Drawn Rod & Bar
Modulus of Elasticity 110 GPa16000 ksiBar, Rod & Forgings
 110 GPa16000 ksiCastings & Strip
 114 GPa16500 ksiPlate
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000203 ohm-cm0.00000203 ohm-cmBar, Rod & Forgings (85 % IACS)
 0.00000216 ohm-cm0.00000216 ohm-cmCastings & Strip (80 % IACS)
 0.00000221 ohm-cm0.00000221 ohm-cmPlate (78 % IACS)
 
Thermal PropertiesMetricEnglishComments
CTE, linear 17.6 µm/m-°C
@Temperature 100 °C
9.78 µin/in-°F
@Temperature 212 °F
Thermal Conductivity 324 W/m-K2250 BTU-in/hr-ft²-°F
Melting Point 1070 - 1075 °C1960 - 1967 °F
Solidus 1070 °C1960 °F
Liquidus 1075 °C1967 °F
Softening Point 500 °C932 °FPermanent Softening
 
Component Elements PropertiesMetricEnglishComments
Chromium, Cr 0.90 %0.90 %
Copper, Cu 99.1 %99.1 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
CMW® 328 Copper Alloy
CMW® 28 Copper Alloy
Chromium Copper, UNS C18500
Chromium Copper, UNS C18400
Cadi 182 Copper Alloy

NCMW066 / 15878

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.