MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Titanium Ti-5Al-5Sn-2Zr-2Mo-0.25Si (Ti-5522S)
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Beta Titanium Alloy

Material Notes: Heat treatment: 975 °C, 1/2 hour, AC and 595 °C, 2 hours, AC

Characteristics: Alpha-beta alloy, good elevated temperature creep properties, good tensile properties, good stress rupture behavior, good thermal stability. Weldable, formable.

Applications: Parts for gas-turbine engines

Key Words: UNS R54560
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 4.52 g/cc0.163 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 32 - 3832 - 38
Tensile Strength 900 - 1048 MPa131000 - 152000 psi
 689 MPa
@Temperature 535 °C
99900 psi
@Temperature 995 °F
Tensile Strength, Yield 830 - 965 MPa120000 - 140000 psi
 517 MPa
@Temperature 535 °C
75000 psi
@Temperature 995 °F
Elongation at Break 10 %10 %
 15 %
@Temperature 535 °C
15 %
@Temperature 995 °F
Reduction of Area 25 %25 %
 35 %
@Temperature 535 °C
35 %
@Temperature 995 °F
Creep Strength >= 345 MPa
@Temperature 510 °C,
Time >=360000 sec
>= 50000 psi
@Temperature 950 °F,
Time >=100 hour
strain 1%
Rupture Strength >= 1170 MPa
@Temperature 23.0 °C,
Time 18000 sec
>= 170000 psi
@Temperature 73.4 °F,
Time 5.00 hour
Notched specimen
Tensile Modulus 113.8 GPa16510 ksi
Poissons Ratio 0.3260.326
Fracture Toughness 82.4 MPa-m½75.0 ksi-in½For forging with yield strength = 890 MPa
Shear Modulus 42.9 GPa6220 ksiCalculated
Charpy Impact 22.0 J16.2 ft-lbnotched
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000171 ohm-cm0.000171 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 10.2 µm/m-°C
@Temperature 20.0 - 815 °C
5.67 µin/in-°F
@Temperature 68.0 - 1500 °F
Melting Point <= 1700 °C<= 3090 °F
Liquidus 1700 °C3090 °F
Beta Transus 980 °C1800 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 4.5 - 5.5 %4.5 - 5.5 %
Carbon, C <= 0.040 %<= 0.040 %
Iron, Fe <= 0.15 %<= 0.15 %
Molybdenum, Mo 1.75 - 2.25 %1.75 - 2.25 %
Nitrogen, N <= 0.030 %<= 0.030 %
Oxygen, O <= 0.13 %<= 0.13 %
Silicon, Si 0.20 - 0.30 %0.20 - 0.30 %
Tin, Sn 4.5 - 5.5 %4.5 - 5.5 %
Titanium, Ti 85 %85 %
Zirconium, Zr 1.75 - 2.25 %1.75 - 2.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-5Al-6Sn-2Zr-1Mo-0.25Si
Titanium Ti-5Al-2Sn-2Zr-4Mo-4Cr (Ti-17) Alpha-Beta Processed
Titanium Ti-6Al-2Sn-2Zr-2Mo-2Cr-.25Si Alpha-Beta Processed + Aged
Titanium Ti-6Al-4V (Grade 5), STA
Titanium IMI 367 (Ti-6Al-7Nb)

MTP5522 / 142956

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.