MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Copper Chloride, CuCl, Cubic (Nantokite)
Categories: Ceramic; Halide; Other Engineering Material; Semiconductor

Key Words: Halide; Semiconductor
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 4.14 g/cc0.150 lb/in³
a Lattice Constant 5.4057 Å5.4057 Å
Formula Units/Cell (Z) 44
Molecular Weight 98.999 g/mol98.999 g/mol
Volume Compressibility, 10^-10 m²/N 0.260.26
 
Mechanical PropertiesMetricEnglishComments
Hardness, Mohs 2.32.3
 
Electrical PropertiesMetricEnglishComments
Magnetic Susceptibility -0.0000400-0.0000400cm^3/mol
Dielectric Constant 7.97.9
Band Gap 3.17 eV3.17 eV
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 110 J/g47.3 BTU/lbCrystal structure not specified.
CTE, linear 12.1 µm/m-°C
@Temperature 20.0 °C
6.72 µin/in-°F
@Temperature 68.0 °F
Specific Heat Capacity 0.490 J/g-°C0.117 BTU/lb-°F
Thermal Conductivity 0.840 W/m-K5.83 BTU-in/hr-ft²-°F
Melting Point 422 °C792 °F
Boiling Point 1400 °C2550 °F
Heat of Formation 481 kJ/mol481 kJ/mol
Debye Temperature -33.0 °C-27.4 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.931.93
 
Descriptive Properties
CAS Number7758-89-6
ColorWhite
Crystal StructureCubicSphalerite Structure - Space Group F(-4)3m

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Copper Chloride, CuCl, Hexagonal
Copper Aluminum Sulfide, CuAlS2
Copper (I) Fluoride, CuF
Copper Bromide, CuBr, Cubic
Copper Antimony Selenide, Cu3SbSe4

DSEM54 / 2969

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.