MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

North American Cherry (Black Cherry) Wood
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: Diffuse-Porous Hardwood. Data is based on small, clear, air-dried samples unless specified.
Usual surface texture: Fine
Dimensional changes when dried lumber is subjected to variations in humidity during service: Medium
Resistance to fungal decay (Heartwood in ground contact): Moderately Durable (10 to 15 years)
Common Applications: Cabinet making, furniture

Key Words: Prunus serotina; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.500 g/cc0.0181 lb/in³Air Dry (12-15% Moisture Content)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 4200 N944 lb (f)Side
Tensile Strength, Ultimate 3.90 MPa566 psiPerpendicular to Grain
Modulus of Rupture 0.0850 GPa12.3 ksiStatic Bending
Flexural Modulus 10.28 GPa1491 ksiStatic Bending
Compressive Strength 5.90 MPa856 psiPerpendicular to Grain
 49.0 MPa7110 psiParallel to Grain
Poissons Ratio 0.0480.048µTL, 12% Moisture Content
 0.0860.086µRL, 12% Moisture Content
 0.2820.282µTR, 12% Moisture Content
 0.3920.392µLR, 12% Moisture Content
 0.4280.428µLT, 12% Moisture Content
 0.6950.695µRT, 12% Moisture Content
Machinability 100 %100 %Good Relative to Other Wood
Shear Strength 11.7 MPa1700 psiOrientation Unknown
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.121 W/m-K0.840 BTU-in/hr-ft²-°FOven Dry
 0.144 W/m-K1.00 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 3.7 %3.7 %Radial; Green to Zero Moisture
 7.1 %7.1 %Tangential; Green to Zero Moisture
 11.5 %11.5 %Volumetric; Green to Zero Moisture
 
Descriptive Properties
ColorReddish-brown to redUsual for heartwood

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
American Red Maple Wood
American Black Ash (Brown Ash) Wood
American White Oak Wood
American Black Walnut Wood
American Chestnut Wood

PTSA090 / 71247

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.