MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Hostaform® S 9362 XAP2 ™ POM, Impact Modified
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, Impact Modified

Material Notes: Preliminary Data Sheet
Drying is suggested to help achieve low emission performance and to counter if material has contacted moisture through improper storage and handling.

Information provided by Celanese Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.39 g/cc0.0502 lb/in³ISO 1183
Water Absorption at Saturation 0.80 %0.80 %ISO 62
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 55.0 MPa7980 psi50mm/min; ISO 527-2/1A
Elongation at Yield 10 %10 %50mm/min; ISO 527-2/1A
Tensile Modulus 2.30 GPa334 ksi1mm/min; ISO 527-2/1A
Flexural Modulus 2.20 GPa319 ksiISO 178
Charpy Impact Unnotched NBNBISO 179/1eU
 19.0 J/cm²
@Temperature -30.0 °C
90.4 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 1.00 J/cm²4.76 ft-lb/in²ISO 179/1eA
 0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.1 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 110 µm/m-°C61.1 µin/in-°FISO 11359-2
Melting Point 166 °C331 °FISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 151 °C304 °FISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 87.0 °C189 °FISO 75-1, -2
 
Processing PropertiesMetricEnglishComments
Processing Temperature 80.0 - 120 °C176 - 248 °Fcavity
Zone 1 170 - 180 °C338 - 356 °F
Zone 2 180 - 190 °C356 - 374 °F
Zone 3 180 - 190 °C356 - 374 °F
Zone 4 180 - 200 °C356 - 392 °F
Die Temperature 180 - 200 °C356 - 392 °F
Melt Temperature 180 - 200 °C356 - 392 °F
Drying Temperature 80.0 - 100 °C176 - 212 °F
Dry Time 3 hour3 hour
Injection Pressure 60.0 - 120 MPa8700 - 17400 psi
Hold Pressure 60.0 - 120 MPa8700 - 17400 psi
Back Pressure <= 0.500 MPa<= 72.5 psi
 
Descriptive Properties
Injection moldingYes
Injection speedslow
Melt volume rate (MVR), cm³/10min6.5
MVR test load, kg2.16
MVR test temperature, °C190
Processing conditions acc. ISO9988-2
Profile extrusionYes
RemarksDo not heat over 205 C (~400 F) to avoid burning and discoloring product.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Hostaform® C 9021 POM, Unfilled
Celanese Hostaform® C 9021 AW XAP² ™ LS POM, Tribological

PHCS402 / 123817

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.