MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Syensqo (Solvay Specialty Polymers) Ixef® 1002 Polyarylamide (PARA), 30% glass fiber
Categories: Polymer; Thermoplastic; Polyarylamide (PAA); Polyarylamide, Glass Fiber Filled

Material Notes: 30% glass fiber, general purpose for injection molding

Ixef® 1002 is a 30% glass-fiber reinforced, general purpose polyarylamide compound which exhibits high strength and rigidity, outstanding surface finish, and excellent creep resistance.

- Black: Ixef® 1002/9008
- Natural: Ixef® 1002/0008
- Custom colorable

Markets/Uses: Automotive / Mechanical & Structural Parts / Accumulator Piston; Air Intake/Lamella; Body Components; Brackets; Brake Power Pistons; / Bushings; Center Drive Assembly; Clutch Cylinder; Door Handles; Door Lock Components; Gas Pedal Support; Engine Mount Orifice; Gears; Poppets; Side Mirror Support; Sunroof Structural Components; Electronics / Mobile Devices Electronic Components / Microspeakers; Microswitches; Battery Covers; Camera Modules; al / Chassis and Frames

Applications: Appliance Components; Appliances; Automotive Applications; Automotive Electronics; Automotive Exterior Parts; Automotive Interior Parts; Automotive Under the Hood; Bushings; Camera Applications; Cell Phones; Electrical Housing; Electrical/Electronic Applications; Furniture; Gears; Industrial Applications; Machine/Mechanical Parts; Metal Replacement; Power/Other Tools

Features: Chemical Resistant; Creep Resistant; Good Dimensional Stability; High Flow; High Stiffness; High Strength; Low Moisture Absorption; Outstanding Surface Finish

Injection notes: Hot runners: 250°C to 260°C (482°F to 500°F)
Storage
- Ixef® compounds are shipped in moisture-resistant packages at moisture levels according to specifications. Sealed, undamaged bags should be preferably stored in a dry room at a maximum temperature of 50°C (122°F) and should be protected from possible damage. If only a portion of a package is used, the remaining material should be transferred into a sealable container. It is recommended that Ixef® resins be dried prior to molding following the recommendations found in this datasheet and/or in the Ixef® processing guide.
Drying
- The material as supplied is ready for molding without drying. However, If the bags have been open for longer than 24 hours, the material needs to be dried. When using a desiccant air dryer with dew point of -28°C (-18°F) or lower, these guidelines can be followed: 0.5-1.5 hour at 120°C (248°F), 1-3 hours at 100°C (212°F), or 1-7 hours at 80°C (176°F).
Injection Molding
- IXEF 1002 compound can be readily injection molded in most screw injection molding machines. A general purpose screw is recommended, with minimum back pressure. The measured melt temperature should be about 280°C (536°F), and the barrel temperatures should be around 250°C to 260°C (482 to 500°F) in the rear zone, gradually increasing to 260 to 290°C (500 to 554°F) in the front zone. If hot runners are used, they should be set to 250 to 260°C (482 to 500°F). To maximize crystallinity, the temperature of the mold cavity surface must be held between 120 and 140°C (248 and 284°F). Molding at lower temperatures will produce articles that may warp, have poor surface appearance, and have a greater tendency to creep. Set injection pressure to give rapid injection. Adjust holding pressure and hold time to maximize part weight. Transfer from injection to hold pressure at the screw position just before the part is completely filled (95-99%).

Information provided by Solvay Specialty Polymers.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.43 g/cc0.0517 lb/in³ISO 1183
Water Absorption 0.20 %
@Time 86400 sec
0.20 %
@Time 24.0 hour
ISO 62
Linear Mold Shrinkage, Flow 0.0010 - 0.0040 cm/cm0.0010 - 0.0040 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 190 MPa27600 psiISO 527-2
Elongation at Break 2.0 %2.0 %ISO 527-2
Tensile Modulus 11.5 GPa1670 ksiISO 527-2
Flexural Strength 285 MPa41300 psiISO 178
Flexural Modulus 11.5 GPa1670 ksiISO 178
Izod Impact, Notched 0.700 J/cm1.31 ft-lb/inASTM D256
Izod Impact, Unnotched 4.60 J/cm8.62 ft-lb/inASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 60093
Dielectric Constant 3.9
@Frequency 110 Hz
3.9
@Frequency 110 Hz
IEC 60250
Dielectric Strength 30.0 kV/mm762 kV/inIEC 60243-1
Dissipation Factor 0.010
@Frequency 110 Hz
0.010
@Frequency 110 Hz
IEC 60250
Comparative Tracking Index 400 V400 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 18.0 µm/m-°C10.0 µin/in-°FISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 230 °C446 °FUnannealed; ISO 75-2/A
Flammability, UL94 HBHB
Oxygen Index 25 %25 %ISO 4589-2
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 250 - 260 °C482 - 500 °F
Front Barrel Temperature 260 - 290 °C500 - 554 °F
Melt Temperature 280 °C536 °FInjection
Mold Temperature 120 - 140 °C248 - 284 °F
Drying Temperature 120 °C
@Time 1800 - 5400 sec
248 °F
@Time 0.500 - 1.50 hour
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorBlack; Colors Available; Natural Color
FormsPellets
Injection RateFast
ProcessingInjection Molding
RoHS ComplianceYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4268 / 280068

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.