MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Refractory Metals

Tungsten, W; Soft Unalloyed
Categories: Metal; Nonferrous Metal; Refractory Metal; Tungsten Alloy; Pure Element

Material Notes: sintered, hot swaged, and annealed 1590ºC

Vendors: Eagle Alloys Corporation is a leading supplier of quality metals and alloys. Our staff prides itself on working fast, efficiently and courteously to get you the information you need. Call (800) 237-9012 or visit www.EagleAlloys.com.

Elmet Technologies is a 100% US owned and operated, fully integrated manufacturer of Molybdenum, Tungsten and related alloys such as TZM, WHA & MoLa. At our 220,000 sqr/ft plant in Lewiston, Maine, Elmet manufactures W & Mo pure powders plus rod, wire, plate, sheet & foil in additional to offering fabrication and machining services. ITAR, ISO and AS9100 registered. www.elmettechnologies.com

PLANSEE SE: Whether it's high temperatures, aggressive chemicals or extreme mechanical loading: PLANSEE supplies a suitable product solution in refractory metals or composite materials. As the world market leader in powder metallurgically produced high performance materials we combine outstanding materials knowledge with profound applications and technology know-how. Visit us at www.plansee.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 19.293 g/cc0.69700 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 3232
Hardness, Vickers 360360
Tensile Strength, Ultimate 620 MPa89900 psi
Tensile Strength, Yield 550 MPa
@Strain 0.2 %
79800 psi
@Strain 0.2 %
Elongation at Break 2.0 %2.0 %
Modulus of Elasticity 415 GPa60200 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000550 ohm-cm0.00000550 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 4.50 µm/m-°C2.50 µin/in-°F
Specific Heat Capacity 0.132 J/g-°C0.0315 BTU/lb-°F
Thermal Conductivity 174 W/m-K1210 BTU-in/hr-ft²-°F
Boiling Point 5555 °C10030 °F
 
Component Elements PropertiesMetricEnglishComments
Tungsten, W 99.95 %99.95 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tungsten, W; Hard Unalloyed
Tungsten, W
Tungsten, W, (drawn wire)
Overview of materials for Tungsten Alloy
Tungsten Alloy A90S

MW900 / 100368

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.