MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 6061-T8
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: Weldability = A; Stress Corrosion Cracking Resistance = A; General Corrosion Resistance = B (A = best; E = worst). General 6061 characteristics and uses: Excellent joining characteristics, good acceptance of applied coatings. Combines relatively high strength, good workability, and high resistance to corrosion; widely available. The T8 and T9 tempers offer better chipping characteristics over the T6 temper.

Uses: Aircraft fittings, camera lens mounts, couplings, marines fittings and hardware, electrical fittings and connectors, decorative or misc. hardware, hinge pins, magneto parts, brake pistons, hydraulic pistons, appliance fittings, valves and valve parts.

Some data provided by Alcoa.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: al6061, Aluminium 6061-T8; UNS A96061; ISO AlMg1SiCu, AD-33 (Russia); AA6061-T8; Al6061-T8
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.70 g/cc0.0975 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 120120500 kg load/10 mm ball
Hardness, Knoop 150150Estimated from Brinell
Hardness, Rockwell A 46.846.8Estimated from Brinell
Hardness, Rockwell B 7575Estimated from Brinell
Hardness, Vickers 136136Estimated from Brinell
Tensile Strength, Ultimate >= 310 MPa>= 45000 psi
Tensile Strength, Yield >= 276 MPa>= 40000 psi
Elongation at Break 8.0 %8.0 %
Modulus of Elasticity 69.0 GPa10000 ksiAverage of Tension and Compression. In Al alloys, the compressive modulus is typically 2% greater than the tensile modulus
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Machinability 50 %50 %0-100 Scale (A=90; B=70; C=50; D=30; E=10)
Shear Modulus 26.0 GPa3770 ksiEstimated from similar Al alloys.
Shear Strength 185 MPa26800 psiEstimated from ultimate tensile strength
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000370 ohm-cm0.00000370 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  23.6 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 25.2 µm/m-°C
@Temperature 20.0 - 300 °C
14.0 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.896 J/g-°C0.214 BTU/lb-°F
Thermal Conductivity 170 W/m-K1180 BTU-in/hr-ft²-°F
Melting Point 582 - 651.7 °C1080 - 1205 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting can be eliminated by homogenization.
Solidus 582 °C1080 °FAA; Typical
Liquidus 651.7 °C1205 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Solution Temperature 529 °C985 °F
Aging Temperature 160 °C320 °FRolled or drawn products; hold at temperature for 18 hr
 177 °C350 °FExtrusions or forgings; hold at temperature for 8 hr
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 95.8 - 98.6 %95.8 - 98.6 %As remainder
Chromium, Cr 0.04 - 0.35 %0.04 - 0.35 %
Copper, Cu 0.15 - 0.40 %0.15 - 0.40 %
Iron, Fe <= 0.70 %<= 0.70 %
Magnesium, Mg 0.80 - 1.2 %0.80 - 1.2 %
Manganese, Mn <= 0.15 %<= 0.15 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 0.40 - 0.80 %0.40 - 0.80 %
Titanium, Ti <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.25 %<= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 6061-T6; 6061-T651
Aluminum 6061-T4; 6061-T451
Aluminum 6061-O
Aluminum 6061-T91
Aluminum 6061-T913

MA6061T8 / 9392

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.