MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Jewelry bronze, UNS C22600, H02 Temper flat products
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Good to excellent corrosion resistance. Excellent cold workability, good hot workability for blanking, coining, drawing, piercing and punching, shearing, spinning, squeezing and swaging, stamping, heading and upsetting, roll threading and knurling.

Applications: angles, channels, chains, fasteners, costume jewelry, lipstick cases, compacts, base for gold plate.

Test specimen: flat products - 1mm thickness.

Key Words: CA226
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.78 g/cc0.317 lb/in³
Grain Size  5.0 µm
@Treatment Temp. 265 °C
5.0 µm
@Treatment Temp. 509 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 7.0 µm
@Treatment Temp. 400 °C
7.0 µm
@Treatment Temp. 752 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 25 µm
@Treatment Temp. 600 °C
25 µm
@Treatment Temp. 1110 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 108 µm
@Treatment Temp. 800 °C
108 µm
@Treatment Temp. 1470 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 120 µm
@Treatment Temp. 825 °C
120 µm
@Treatment Temp. 1520 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 6161
Tensile Strength, Ultimate 370 MPa53700 psi
 260 MPa
@Treatment Temp. 800 °C
37700 psi
@Treatment Temp. 1470 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 270 MPa
@Treatment Temp. 600 °C
39200 psi
@Treatment Temp. 1110 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 310 MPa
@Treatment Temp. 400 °C
45000 psi
@Treatment Temp. 752 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 400 MPa
@Treatment Temp. 320 °C
58000 psi
@Treatment Temp. 608 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 490 MPa
@Treatment Temp. 200 °C
71100 psi
@Treatment Temp. 392 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
Tensile Strength, Yield 325 MPa47100 psi
Elongation at Break 12 %12 %In 50 mm
 6.0 %
@Treatment Temp. 200 °C
6.0 %
@Treatment Temp. 392 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 20 %
@Treatment Temp. 330 °C
20 %
@Treatment Temp. 626 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 42 %
@Treatment Temp. 400 °C
42 %
@Treatment Temp. 752 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 46 %
@Treatment Temp. 800 °C
46 %
@Treatment Temp. 1470 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
 49 %
@Treatment Temp. 600 °C
49 %
@Treatment Temp. 1110 °F
strip with initial grain size of 0.035 mm, cold rolled 50% to 1 mm thick, annealed 1h
Modulus of Elasticity 115 GPa16700 ksi
Poissons Ratio 0.3070.307
Machinability 30 %30 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 44.0 GPa6380 ksi
Shear Strength 250 MPa36300 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000430 ohm-cm
@Temperature 20.0 °C
0.00000430 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.6 µm/m-°C
@Temperature 20.0 - 300 °C
10.3 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.380 J/g-°C0.0908 BTU/lb-°F
Thermal Conductivity 173 W/m-K
@Temperature 20.0 °C
1200 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1005 - 1035 °C1841 - 1895 °F
Solidus 1005 °C1841 °F
Liquidus 1035 °C1895 °F
Annealing Point 427 - 760 °C800 - 1400 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 425 - 750 °C797 - 1380 °F
Hot-Working Temperature 750 - 900 °C1380 - 1650 °F
Recrystallization Temperature 330 °C
@Thickness 1.00 mm
626 °F
@Thickness 0.0394 in
Approximately
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 86 - 89 %86 - 89 %
Iron, Fe >= 0.0050 %>= 0.0050 %
Lead, Pb >= 0.050 %>= 0.050 %
Zinc, Zn 12.5 %12.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Jewelry bronze, UNS C22600, H01 Temper flat products
Copper, UNS C27000 (Yellow brass), H01 Temper flat products
Copper, UNS C26800 (Yellow brass), OSO15 Temper flat products
Copper, UNS C26800 (Yellow brass), OSO50 Temper flat products
Copper, UNS C26800 (Yellow brass), H01 Temper flat products

MC22600b8 / 11019

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.