MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

TIMET TIMETAL® 65A CP Titanium (ASTM Grade 3)
Categories: Metal; Nonferrous Metal; Titanium Alloy; Unalloyed/Modified Titanium

Material Notes: Commercially Pure Titanium.

Industry Specifications: USA Aerospace: AMS 4900. Germany Aerospace: 3.7055. France: T-50. UK Aerospace Specification DTD 5023, 5273.

Features: The mechanical properties of CP titanium are influenced by small additions of oxygen and iron. By careful control of these additions, the various grades of commercially pure titanium are produced to give properties suited to different applications. TIMETAL 65A is equivalent to ASTM Grade 3. It is a general purpose grade of commercially pure titanium that has excellent corrosion resistance in highly oxidizing to mildly reducing environments, including chlorides, and an excellent strength to weight ratio. It offers the highest ASME allowable design stresses of any commercially pure grade of titanium. 65A also has good impact properties at low temperatures. It can be satisfactorily welded, machined, cold worked, hot worked, and cast. It is nonmagnetic.

Typical heat treatment for this alloy: Anneal at 700°C for 1 hour and air cool. Stress Relieve at 500°C for 30 mins and air cool.

Data provided by TIMET.

Key Words: UNS R50550
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.51 g/cc0.163 lb/in³Typical
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 585 MPa84800 psiTypical
 174 MPa
@Temperature 450 °C
25200 psi
@Temperature 842 °F
 195 MPa
@Temperature 400 °C
28300 psi
@Temperature 752 °F
 250 MPa
@Temperature 300 °C
36300 psi
@Temperature 572 °F
 327 MPa
@Temperature 200 °C
47400 psi
@Temperature 392 °F
 438 MPa
@Temperature 100 °C
63500 psi
@Temperature 212 °F
Tensile Strength, Yield 450 MPa
@Strain 0.2 %
65300 psi
@Strain 0.2 %
Typical
 92.0 MPa
@Strain 0.2 %,
Temperature 450 °C
13300 psi
@Strain 0.2 %,
Temperature 842 °F
 101 MPa
@Strain 0.2 %,
Temperature 400 °C
14600 psi
@Strain 0.2 %,
Temperature 752 °F
 129 MPa
@Strain 0.2 %,
Temperature 300 °C
18700 psi
@Strain 0.2 %,
Temperature 572 °F
 195 MPa
@Strain 0.2 %,
Temperature 200 °C
28300 psi
@Strain 0.2 %,
Temperature 392 °F
 283 MPa
@Strain 0.2 %,
Temperature 100 °C
41000 psi
@Strain 0.2 %,
Temperature 212 °F
Elongation at Break 25 %25 %Typical
 31 %
@Temperature 100 °C
31 %
@Temperature 212 °F
 33 %
@Temperature 400 °C
33 %
@Temperature 752 °F
 36 %
@Temperature 200 °C
36 %
@Temperature 392 °F
 39 %
@Temperature 300 °C
39 %
@Temperature 572 °F
Reduction of Area 48 %48 %Typical
Modulus of Elasticity 105 - 120 GPa15200 - 17400 ksiTypical
Fatigue Strength  116 MPa
@# of Cycles 1.00e+7
16800 psi
@# of Cycles 1.00e+7
Notched, Kt=4; rotating bend (sample with UTS = 589 MPa)
 116 MPa
@# of Cycles 1.00e+7
16800 psi
@# of Cycles 1.00e+7
Notched, Kt=3.3; rotating bend (sample with UTS = 550 MPa)
 123 MPa
@# of Cycles 1.00e+7
17800 psi
@# of Cycles 1.00e+7
Notched, Kt=3; rotating bend (sample with UTS = 589 MPa)
 147 MPa
@# of Cycles 1.00e+7
21300 psi
@# of Cycles 1.00e+7
Notched, Kt=2; rotating bend (sample with UTS = 589 MPa)
 170 MPa
@# of Cycles 1.00e+7
24700 psi
@# of Cycles 1.00e+7
Notched, Kt=2; rotating bend (sample with UTS = 550 MPa)
 247 MPa
@# of Cycles 1.00e+7
35800 psi
@# of Cycles 1.00e+7
Notched, Kt=1.5; rotating bend (sample with UTS = 550 MPa)
 263 MPa
@# of Cycles 1.00e+7
38100 psi
@# of Cycles 1.00e+7
Smooth, Kt=1; rotating bend (sample with UTS = 550 Mpa)
 278 MPa
@# of Cycles 1.00e+7
40300 psi
@# of Cycles 1.00e+7
Smooth, Kt=1; rotating bend (sample with UTS = 589 Mpa)
Bend Radius, Minimum 2.5 t
@Thickness 2.00 mm
2.5 t
@Thickness 0.0787 in
Typical; sheet
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000540 ohm-cm0.0000540 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  8.60 µm/m-°C
@Temperature 20.0 - 100 °C
4.78 µin/in-°F
@Temperature 68.0 - 212 °F
 9.50 µm/m-°C
@Temperature 20.0 - 300 °C
5.28 µin/in-°F
@Temperature 68.0 - 572 °F
 9.70 µm/m-°C
@Temperature 20.0 - 500 °C
5.39 µin/in-°F
@Temperature 68.0 - 932 °F
Thermal Conductivity 21.79 W/m-K151.2 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 425 °C797 °FContinuous
 540 °C1000 °FIntermittent
Beta Transus 920 °C1690 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe <= 0.30 %<= 0.30 %
Nitrogen, N <= 0.050 %<= 0.050 %
Oxygen, O <= 0.35 %<= 0.35 %
Titanium, Ti >= 98.8 %>= 98.8 %As Remainder

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Grade 3
TIMET 75A CP Titanium (ASTM Grade 4)
Titanium Grade 4, Annealed
Titanium Grade 3, Annealed
ASTM A36 Steel, bar

NTIME65A / 19333

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.