MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Oxygen-free Electronic Copper (OFE), UNS C10100, H80 (16%) Temper, rod
Categories: Metal; Nonferrous Metal; Copper Alloy; Wrought Copper

Material Notes: Test specimen: rod, 50mm diam.

Applications: busbars, bus conductors, waveguides, hollow conductors, lead-in wires and anodes for vacuum tubes, vacuum seals, transistor components, glass-to-metal seals, coaxial cables, klystrons, microwave tubes, and rectifiers.

Processing: Excellent hot and cold workability; good forgeability. Fabricated by bending, coining, coppersmithing, drawing and upsetting, hot forging and pressing, knurling, roll threading, shearing, spinning, swaging, and stamping.

Corrosion Resistance: Good to excellent. Susceptible to galvanic corrosion when coupled with iron, aluminum, magnesium, lead, tin, and zinc. Good resistance to atmospheric, brackish water, sea water, and non-oxidizing acid corrosion, but avoid heating in oxidizing atmospheres or exposing to oxidizing acids, moist halogens, sulfides, ammonia, or solutions with ammonium ions.

UNS C10100 - ASTM B12, B49,B133, B187, F 68; 101A (Australia); C110 (UK); CDA 101 OFE; ISO Cu-OFE; JIS C1011 H3510 (Japan); QQ-C-502

Key Words: ASTM B12, B49, B133, B187, F68, AS 101A 1567 (Australia), Cu/cl NF A53301 (France), ISO Cu-OFE, CEN CW009A, oxygen-free high conductivity copper (OFHC), JIS C1011 H3510, QQ-C-502, CDA 101 OFE
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.94 g/cc0.323 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 4545
Hardness, Rockwell F 8585
Tensile Strength, Ultimate 310 MPa45000 psi
 10.0 MPa
@Temperature 800 °C
1450 psi
@Temperature 1470 °F
 15.0 MPa
@Temperature 700 °C
2180 psi
@Temperature 1290 °F
 35.0 MPa
@Temperature 600 °C
5080 psi
@Temperature 1110 °F
 60.0 MPa
@Temperature 500 °C
8700 psi
@Temperature 932 °F
 150 MPa
@Temperature 400 °C
21800 psi
@Temperature 752 °F
 260 MPa
@Temperature 300 °C
37700 psi
@Temperature 572 °F
 340 MPa
@Temperature 200 °C
49300 psi
@Temperature 392 °F
 350 MPa
@Temperature 0.000 °C
50800 psi
@Temperature 32.0 °F
bar
 360 MPa
@Temperature -50.0 °C
52200 psi
@Temperature -58.0 °F
bar
 375 MPa
@Temperature -100 °C
54400 psi
@Temperature -148 °F
bar
 390 MPa
@Temperature 100 °C
56600 psi
@Temperature 212 °F
 420 MPa
@Temperature -150 °C
60900 psi
@Temperature -238 °F
bar
 435 MPa
@Temperature 20.0 °C
63100 psi
@Temperature 68.0 °F
 470 MPa
@Temperature -200 °C
68200 psi
@Temperature -328 °F
bar
 530 MPa
@Temperature -250 °C
76900 psi
@Temperature -418 °F
bar
Tensile Strength, Yield 275 MPa
@Strain 0.5 %
39900 psi
@Strain 0.5 %
 1.00 MPa
@Strain 0.2 %,
Temperature 800 °C
145 psi
@Strain 0.2 %,
Temperature 1470 °F
 2.00 MPa
@Strain 0.2 %,
Temperature 700 °C
290 psi
@Strain 0.2 %,
Temperature 1290 °F
 10.0 MPa
@Strain 0.2 %,
Temperature 600 °C
1450 psi
@Strain 0.2 %,
Temperature 1110 °F
 25.0 MPa
@Strain 0.2 %,
Temperature 500 °C
3630 psi
@Strain 0.2 %,
Temperature 932 °F
 125 MPa
@Strain 0.2 %,
Temperature 400 °C
18100 psi
@Strain 0.2 %,
Temperature 752 °F
 250 MPa
@Strain 0.2 %,
Temperature 300 °C
36300 psi
@Strain 0.2 %,
Temperature 572 °F
 325 MPa
@Strain 0.2 %,
Temperature 200 °C
47100 psi
@Strain 0.2 %,
Temperature 392 °F
 325 MPa
@Strain 0.2 %,
Temperature -50.0 °C
47100 psi
@Strain 0.2 %,
Temperature -58.0 °F
bar
 325 MPa
@Strain 0.2 %,
Temperature 0.000 °C
47100 psi
@Strain 0.2 %,
Temperature 32.0 °F
bar
 330 MPa
@Strain 0.2 %,
Temperature -100 °C
47900 psi
@Strain 0.2 %,
Temperature -148 °F
bar
 345 MPa
@Strain 0.2 %,
Temperature -150 °C
50000 psi
@Strain 0.2 %,
Temperature -238 °F
bar
 370 MPa
@Strain 0.2 %,
Temperature -200 °C
53700 psi
@Strain 0.2 %,
Temperature -328 °F
bar
 380 MPa
@Strain 0.2 %,
Temperature 100 °C
55100 psi
@Strain 0.2 %,
Temperature 212 °F
 390 MPa
@Strain 0.2 %,
Temperature -250 °C
56600 psi
@Strain 0.2 %,
Temperature -418 °F
bar
 420 MPa
@Strain 0.2 %,
Temperature 20.0 °C
60900 psi
@Strain 0.2 %,
Temperature 68.0 °F
Elongation at Break 20 %20 %in 50 mm (2 in)
 17 %
@Temperature 200 °C
17 %
@Temperature 392 °F
 17 %
@Temperature -50.0 °C
17 %
@Temperature -58.0 °F
bar
 17 %
@Temperature 0.000 °C
17 %
@Temperature 32.0 °F
bar
 19 %
@Temperature -100 °C
19 %
@Temperature -148 °F
bar
 23 %
@Temperature 300 °C
23 %
@Temperature 572 °F
 24 %
@Temperature 100 °C
24 %
@Temperature 212 °F
 24 %
@Temperature -150 °C
24 %
@Temperature -238 °F
bar
 27 %
@Temperature 20.0 °C
27 %
@Temperature 68.0 °F
 31 %
@Temperature -200 °C
31 %
@Temperature -328 °F
bar
 37 %
@Temperature 400 °C
37 %
@Temperature 752 °F
 42 %
@Temperature -250 °C
42 %
@Temperature -418 °F
bar
 46 %
@Temperature 500 °C
46 %
@Temperature 932 °F
 48 %
@Temperature 600 °C
48 %
@Temperature 1110 °F
 53 %
@Temperature 700 °C
53 %
@Temperature 1290 °F
 60 %
@Temperature 800 °C
60 %
@Temperature 1470 °F
Reduction of Area  35 %
@Temperature 300 °C
35 %
@Temperature 572 °F
 38 %
@Temperature 200 °C
38 %
@Temperature 392 °F
 57 %
@Temperature 400 °C
57 %
@Temperature 752 °F
 67 %
@Temperature 100 °C
67 %
@Temperature 212 °F
 73 %
@Temperature 500 °C
73 %
@Temperature 932 °F
 80 %
@Temperature 20.0 °C
80 %
@Temperature 68.0 °F
 82 %
@Temperature 600 °C
82 %
@Temperature 1110 °F
 90 %
@Temperature 700 °C
90 %
@Temperature 1290 °F
 95 %
@Temperature 800 °C
95 %
@Temperature 1470 °F
Rupture Strength  5.20 MPa
@Temperature 650 °C,
Time 360000 sec
754 psi
@Temperature 1200 °F,
Time 100 hour
 9.70 MPa
@Temperature 650 °C,
Time 36000 sec
1410 psi
@Temperature 1200 °F,
Time 10.0 hour
 17.0 MPa
@Temperature 450 °C,
Time 360000 sec
2470 psi
@Temperature 842 °F,
Time 100 hour
 33.0 MPa
@Temperature 450 °C,
Time 36000 sec
4790 psi
@Temperature 842 °F,
Time 10.0 hour
Modulus of Elasticity 115 GPa16700 ksi
Poissons Ratio 0.310.31
Machinability 20 %20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 65 %65 %UNS C37700 (forging brass) = 100%
Shear Modulus 44.0 GPa6380 ksi
Shear Strength 180 MPa26100 psi
Charpy Impact  118 J
@Temperature -250 °C
87.0 ft-lb
@Temperature -418 °F
bar; V-notch
 132 J
@Temperature -200 °C
97.4 ft-lb
@Temperature -328 °F
bar; V-notch
 135 J
@Temperature 0.000 °C
99.6 ft-lb
@Temperature 32.0 °F
bar; V-notch
 138 J
@Temperature -150 °C
102 ft-lb
@Temperature -238 °F
bar; V-notch
 139 J
@Temperature -50.0 °C
103 ft-lb
@Temperature -58.0 °F
bar; V-notch
 140 J
@Temperature -100 °C
103 ft-lb
@Temperature -148 °F
bar; V-notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000171 ohm-cm
@Temperature 20.0 °C
0.00000171 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  17.0 µm/m-°C
@Temperature 20.0 - 100 °C
9.44 µin/in-°F
@Temperature 68.0 - 212 °F
 17.3 µm/m-°C
@Temperature 20.0 - 200 °C
9.61 µin/in-°F
@Temperature 68.0 - 392 °F
 17.7 µm/m-°C
@Temperature 20.0 - 300 °C
9.83 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.385 J/g-°C
@Temperature 20.0 °C
0.0920 BTU/lb-°F
@Temperature 68.0 °F
Thermal Conductivity 391 W/m-K
@Temperature 20.0 °C
2710 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1083 °C1981 °F
Annealing Point >= 371 °C>= 700 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 375 - 650 °C707 - 1200 °F
Hot-Working Temperature 750 - 875 °C1380 - 1610 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu >= 99.99 %>= 99.99 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Oxygen-free Electronic Copper (OFE), UNS C10100, H80 (35%), rod (25 mm Diameter)
Oxygen-free high conductivity Copper, Soft, UNS C10200
Oxygen-free Electronic Copper (OFE), UNS C10100, H80 (15%) temper, shapes
Oxygen-free Electronic Copper (OFE), UNS C10100, O61 Temper Bar
Oxygen-free electronic Copper, UNS C10100

MC10100c4 / 10361

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.