MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Caribbean Pitch Pine (Sapwood) Wood
Categories: Wood and Natural Products; Wood; Softwood

Material Notes: Test material of Honduras origin.

Key Words: Pinus caribaea; P.spp.; Sandlewood; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.680 g/cc0.680 g/ccGreen
Density 0.414 - 0.539 g/cc0.0150 - 0.0195 lb/in³at nominal specific gravity
 0.459 - 0.588 g/cc0.0166 - 0.0212 lb/in³at oven-dry state
 0.495 - 0.637 g/cc0.0179 - 0.0230 lb/in³at 13.5% m.c.
 0.591 g/cc0.0214 lb/in³Nominal; at 13.5% m.c.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 4400 N989 lb (f)Side Hardness, Green
 5500 N1240 lb (f)Side Hardness, 12% Moisture
Modulus of Rupture 0.0772 GPa11.2 ksiStatic Bending, Green
 0.1151 GPa16.69 ksiStatic Bending, 12% Moisture
Flexural Modulus 13.0 GPa1890 ksiStatic Bending, Green
 15.4 GPa2230 ksiStatic Bending, 12% Moisture
Compressive Strength 33.8 MPa4900 psiParallel to Grain, Green
 58.9 MPa8540 psiParallel to Grain, 12% Moisture
Shear Strength 8.10 MPa1170 psiParallel to Grain, Green
 14.4 MPa2090 psiParallel to Grain, 12% Moisture
Work to Maximum Load 0.0740 J/cm³10.7 in-lb/in³Static Bending, Green
 0.119 J/cm³17.3 in-lb/in³Static Bending, 12% Moisture
 
Thermal PropertiesMetricEnglishComments
Shrinkage 6.3 %6.3 %Radial Shrinkage Green to Oven Dry
 7.8 %7.8 %Tangential Shrinkage Green to Oven Dry
 12.9 %12.9 %Volumetric Shrinkage Green to Oven Dry

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lodgepole Pine Wood
Northern White Pine Wood
European Scots Pine Wood
Canadian Spruce Wood
Pitch Pine Wood

PTSM003 / 71356

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.