MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Eastman Tenite 307A4000018 Propionate Clear, Trsp  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Cellulosic; Cellulose Acetate Propionate, Molded

Material Notes: Tenite cellulosic plastics are noted for their excellent balance of properties - toughness, hardness, strength, surface gloss, clarity, and a warm feel. The mechanical properties of Tenite cellulosic plastics differ with plasticizer levels. Lower plasticizer content yields a harder surface, higher heat resistance, greater rigidity, higher tensile strength, and better dimensional stability. Higher plasticizer content increases impact strength. Tenite cellulosic plastics are available in natural, clear, selected ambers or smoke transparents and black translucent. Color concentrates are available in let-down ratios from 10:1 to 40:1. Tenite Cellulosic Acetate Propionate 307-18 has a plasticizer level of 18%. It is resistant to high temperatures.

Applications/Uses

  • Ophthalmic
  • Optical safety frames
  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Specific Gravity 1.19 g/cc1.19 g/ccASTM D792
    Water Absorption 1.4 %1.4 %24h Immersion; ASTM D570
    Linear Mold Shrinkage 0.0020 - 0.0060 cm/cm0.0020 - 0.0060 in/inASTM D955
    Collected Volatile Condensable Material 1.0 %1.0 %Weight loss on heating, 72hrs, 80°C; ASTM D707
     
    Mechanical PropertiesMetricEnglishComments
    Tensile Strength at Break 27.6 MPa4000 psiASTM D638
    Tensile Strength, Yield 22.1 MPa3210 psiASTM D638
    Elongation at Break 35 %35 %ASTM D638
    Flexural Yield Strength 29.0 MPa4210 psiASTM D790
    Flexural Modulus 1.172 GPa170.0 ksiASTM D790
    Izod Impact, Notched  1.07 J/cm
    @Temperature -40.0 °C
    2.00 ft-lb/in
    @Temperature -40.0 °F
    ASTM D256
     5.23 J/cm
    @Temperature 23.0 °C
    9.80 ft-lb/in
    @Temperature 73.4 °F
    ASTM D256
     
    Electrical PropertiesMetricEnglishComments
    Volume Resistivity 1.00e+13 - 1.00e+15 ohm-cm1.00e+13 - 1.00e+15 ohm-cmASTM D257
    Dielectric Constant 3.3 - 3.8
    @Frequency 1e+6 Hz
    3.3 - 3.8
    @Frequency 1e+6 Hz
    ASTM D150
    Dielectric Strength 11.8 - 18.7 kV/mm300 - 475 kV/inASTM D149
    Dissipation Factor 0.010 - 0.15
    @Frequency 1e+6 Hz
    0.010 - 0.15
    @Frequency 1e+6 Hz
    ASTM D150
     
    Thermal PropertiesMetricEnglishComments
    CTE, linear 110 - 170 µm/m-°C
    @Temperature 20.0 °C
    61.1 - 94.4 µin/in-°F
    @Temperature 68.0 °F
    ASTM D696
    Specific Heat Capacity 1.26 - 1.67 J/g-°C0.301 - 0.399 BTU/lb-°FDSC
    Thermal Conductivity 0.170 - 0.330 W/m-K1.18 - 2.29 BTU-in/hr-ft²-°FASTM C177
    Deflection Temperature at 0.46 MPa (66 psi) 77.0 °C171 °FASTM D648
    Deflection Temperature at 1.8 MPa (264 psi) 67.0 °C153 °FASTM D648
    Vicat Softening Point 87.0 °C189 °FASTM D1525
     
    Optical PropertiesMetricEnglishComments
    Refractive Index 1.46 - 1.49
    @Wavelength 589.3 nm
    1.46 - 1.49
    @Wavelength 589.3 nm
    nD; ASTM D542
    Haze <= 8.5 %<= 8.5 %ASTM D1003
    Transmission, Visible >= 90 %
    @Thickness 1.52 mm
    >= 90 %
    @Thickness 0.0598 in
    ASTM D1003
     
    Descriptive Properties
    Plasticizer, %18
    Soluble Matter Loss, %0.1ASTM D570

    **
    Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

    Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Eastman Tenite 360E461312 Propionate Clear, Trsp
    Eastman Tenite 285E3720005 Butyrate Clear, Trsp
    Eastman Tenite 105E3V36327 Acetate Clear, Trsp
    Eastman Tenite 307A4000015 Propionate Clear, Trsp
    Overview of materials for Nylon 612, Unreinforced

    PE9106 / 35162

    Aluminum Castings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.