Physical Properties | Metric | English | Comments |
---|
Density | 2.80 g/cc | 0.101 lb/in³ |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 6.05 µm/m-°C | 3.36 µin/in-°F |
Softening Point | 705 °C | 1300 °F |
Annealing Point | 545 °C | 1010 °F |
Strain Point | 705 °C | 1300 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.59692 @Wavelength 656.3 nm | 1.59692 @Wavelength 656.3 nm |
| 1.59957 @Wavelength 643.8 nm | 1.59957 @Wavelength 643.8 nm |
| 1.60090 @Wavelength 587.6 nm | 1.60090 @Wavelength 587.6 nm |
| 1.604 @Wavelength 546.1 nm | 1.604 @Wavelength 546.1 nm |
| 1.61004 @Wavelength 486.1 nm | 1.61004 @Wavelength 486.1 nm |
| 1.61081 @Wavelength 480 nm | 1.61081 @Wavelength 480 nm |
Abbe Number | 45.5 | 45.5 |
| 45.7 | 45.7 |
Transmission, Visible | 22 % @Wavelength 380 - 500 nm, Thickness 2.00 mm | 22 % @Wavelength 380 - 500 nm, Thickness 0.0787 in |
| 29 % @Wavelength 380 - 780 nm, Thickness 2.00 mm | 29 % @Wavelength 380 - 780 nm, Thickness 0.0787 in |
| 81 % @Wavelength 380 - 500 nm, Thickness 2.00 mm | 81 % @Wavelength 380 - 500 nm, Thickness 0.0787 in |
| 88 % @Wavelength 380 - 780 nm, Thickness 2.00 mm | 88 % @Wavelength 380 - 780 nm, Thickness 0.0787 in |
UV Transmittance | <= 0.10 % @Thickness 2.00 mm | <= 0.10 % @Thickness 0.0787 in |
| <= 0.10 % @Thickness 2.00 mm | <= 0.10 % @Thickness 0.0787 in |
| 1.5 % @Thickness 2.00 mm | 1.5 % @Thickness 0.0787 in |
| 6.5 % @Thickness 2.00 mm | 6.5 % @Thickness 0.0787 in |
| <= 0.10 % @Wavelength 280 - 315 nm, Thickness 2.00 mm | <= 0.10 % @Wavelength 280 - 315 nm, Thickness 0.0787 in |
| <= 0.10 % @Wavelength 280 - 315 nm, Thickness 2.00 mm | <= 0.10 % @Wavelength 280 - 315 nm, Thickness 0.0787 in |
| <= 0.10 % @Wavelength 280 - 315 nm, Thickness 2.00 mm | <= 0.10 % @Wavelength 280 - 315 nm, Thickness 0.0787 in |
| <= 0.10 % @Wavelength 280 - 315 nm, Thickness 2.00 mm | <= 0.10 % @Wavelength 280 - 315 nm, Thickness 0.0787 in |
| 1.5 % @Wavelength 315 - 350 nm, Thickness 2.00 mm | 1.5 % @Wavelength 315 - 350 nm, Thickness 0.0787 in |
| 2.5 % @Wavelength 380 - 500 nm, Thickness 2.00 mm | 2.5 % @Wavelength 380 - 500 nm, Thickness 0.0787 in |
| 5.5 % @Wavelength 315 - 350 nm, Thickness 2.00 mm | 5.5 % @Wavelength 315 - 350 nm, Thickness 0.0787 in |
| 9.5 % @Wavelength 380 - 500 nm, Thickness 2.00 mm | 9.5 % @Wavelength 380 - 500 nm, Thickness 0.0787 in |
|
Descriptive Properties |
---|
Color | Clear to medium brown |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.