MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Asahi Kasei Leona™ 14G25 Polyamide 66, Heat Stabilized, GF Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: Applications: Mechanical and electrical parts, engine mounts and other under-the-hood automotive parts

Information provided by Asahi Kasei Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.32 g/cc1.32 g/ccDry as Molded; ASTM D792
Density 1.32 g/cc0.0477 lb/in³Dry as Molded; ISO 1183
Moisture Absorption at Equilibrium  1.9 %
@Temperature 23.0 °C
1.9 %
@Temperature 73.4 °F
50% RH; ISO 62
 1.9 %
@Temperature 23.0 °C
1.9 %
@Temperature 73.4 °F
50% RH
Linear Mold Shrinkage, Flow >= 0.0050 cm/cm>= 0.0050 in/inAsahi Kasei
Linear Mold Shrinkage, Transverse >= 0.0090 cm/cm>= 0.0090 in/inAsahi Kasei
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7474Conditioned at 50% RH; ISO 2039
 9696Dry as Molded; ISO 2039
Hardness, Rockwell R 120120Dry as Molded; ISO 2039
Tensile Strength at Break 112 MPa16200 psiConditioned at 50% RH; ISO 527
 190 MPa27600 psiDry as Molded; ISO 527
Tensile Strength 110 MPa16000 psiConditioned at 50% RH; ASTM D638
 180 MPa26100 psiDry as Molded; ASTM D638
Tensile Strength, Yield 116 MPa16800 psiConditioned at 50% RH; ISO 527
Elongation at Break 4.0 %4.0 %Dry as Molded; ISO 527
 9.0 %9.0 %Conditioned at 50% RH; ISO 527
Elongation at Yield 5.5 %
@Temperature 23.0 °C
5.5 %
@Temperature 73.4 °F
Conditioned at 50% RH; ISO 527
Tensile Modulus 5.90 GPa856 ksiDry as Molded; ISO 527
 8.20 GPa1190 ksiConditioned at 50% RH; ISO 527
Flexural Strength 170 MPa24700 psiConditioned at 50% RH; ISO 178
 275 MPa39900 psiDry as Molded; ISO 178
Flexural Modulus 5.00 GPa725 ksiConditioned at 50% RH; ISO 178
 7.80 GPa1130 ksiDry as Molded; ISO 178
Izod Impact, Notched 1.05 J/cm1.97 ft-lb/inDry as Molded; ASTM D256
 1.80 J/cm3.37 ft-lb/inConditioned at 50% RH; ASTM D256
Charpy Impact Unnotched 6.80 J/cm²32.4 ft-lb/in²Dry as Molded; ISO 179
 9.20 J/cm²43.8 ft-lb/in²Conditioned at 50% RH; ISO 179
Charpy Impact, Notched 1.00 J/cm²4.76 ft-lb/in²Dry as Molded; ISO 179
 1.40 J/cm²6.66 ft-lb/in²Conditioned at 50% RH; ISO 179
Taber Abrasion, mg/1000 Cycles 1212Conditioned at 50% RH; ASTM D1044
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmDry as Molded; IEC 60093
Surface Resistance 1.00e+15 ohm1.00e+15 ohmDry as Molded; IEC 60093
Dielectric Strength 29.0 kV/mm737 kV/inDry as Molded; IEC 60243
Comparative Tracking Index 425 V
@Thickness 3.00 mm
425 V
@Thickness 0.118 in
Dry as Molded; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 30.0 µm/m-°C16.7 µin/in-°FDry as Molded; ASTMD 696
Thermal Conductivity 0.300 W/m-K2.08 BTU-in/hr-ft²-°FDry as Molded
Deflection Temperature at 0.46 MPa (66 psi) 260 °C500 °FDry as Molded; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 245 °C473 °FDry as Molded; ISO 75
Flammability, UL94 HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
Dry as Molded

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lubrizol ISOPLAST™ 302EZ Engineering Thermoplastic Polyurethane Resin
Evonik VESTAKEEP® 1000P PEEK
Envalior Stanyl® TE341 Nylon 46 (European Grade) (Dry)
Covestro Makroblend® UT-640 G Polycarbonate + Polyester Blend
BASF Ultrason® E 2010 SW Q31 10088 PESU

PASAHI8136 / 221163

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.