MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polyphenylene Ether, 20% Glass Filled
Categories: Polymer; Thermoplastic; Polyphenylene Ether/PPO; Polyphenylene Ether, 20% Glass Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyphenylene Ether, 20% Glass Filled". Specific grades with glass content between 15% and 24% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.15 - 1.32 g/cc0.0415 - 0.0477 lb/in³Average value: 1.22 g/cc Grade Count:46
Filler Content 20.0 %20.0 %Average value: 20.0 % Grade Count:7
Water Absorption 0.000 - 0.500 %0.000 - 0.500 %Average value: 0.0996 % Grade Count:24
Linear Mold Shrinkage 0.00100 - 0.0110 cm/cm0.00100 - 0.0110 in/inAverage value: 0.00363 cm/cm Grade Count:36
Linear Mold Shrinkage, Transverse 0.00200 - 0.00800 cm/cm0.00200 - 0.00800 in/inAverage value: 0.00462 cm/cm Grade Count:13
Melt Flow 1.00 - 50.0 g/10 min1.00 - 50.0 g/10 minAverage value: 14.8 g/10 min Grade Count:23
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell L 105 - 112105 - 112Average value: 108 Grade Count:3
Hardness, Rockwell R 106 - 118106 - 118Average value: 110 Grade Count:3
Tensile Strength, Ultimate 55.2 - 123 MPa8000 - 17800 psiAverage value: 92.1 MPa Grade Count:38
 20.0 - 70.0 MPa
@Temperature 60.0 - 120 °C
2900 - 10200 psi
@Temperature 140 - 248 °F
Average value: 44.2 MPa Grade Count:2
Tensile Strength, Yield 80.0 - 118 MPa11600 - 17100 psiAverage value: 96.8 MPa Grade Count:12
Elongation at Break 1.00 - 10.0 %1.00 - 10.0 %Average value: 3.52 % Grade Count:37
 2.00 - 4.00 %
@Temperature 60.0 - 120 °C
2.00 - 4.00 %
@Temperature 140 - 248 °F
Average value: 2.70 % Grade Count:2
Elongation at Yield 1.50 - 2.00 %
@Temperature 60.0 - 120 °C
1.50 - 2.00 %
@Temperature 140 - 248 °F
Average value: 1.70 % Grade Count:2
Modulus of Elasticity 3.10 - 7.00 GPa450 - 1020 ksiAverage value: 6.22 GPa Grade Count:20
 3.30 - 6.30 GPa
@Temperature 60.0 - 120 °C
479 - 914 ksi
@Temperature 140 - 248 °F
Average value: 5.17 GPa Grade Count:2
Flexural Yield Strength 96.5 - 194 MPa14000 - 28200 psiAverage value: 136 MPa Grade Count:31
Flexural Modulus 3.20 - 6.50 GPa464 - 943 ksiAverage value: 5.18 GPa Grade Count:41
Izod Impact, Notched 0.534 - 1.20 J/cm1.00 - 2.25 ft-lb/inAverage value: 0.916 J/cm Grade Count:28
 0.5339 - 0.90763 J/cm
@Temperature -40.0 - -30.0 °C
1.000 - 1.7004 ft-lb/in
@Temperature -40.0 - -22.0 °F
Average value: 0.697 J/cm Grade Count:4
 0.600 - 0.700 J/cm
@Temperature -30.0 - 0.000 °C
1.12 - 1.31 ft-lb/in
@Temperature -22.0 - 32.0 °F
Average value: 0.697 J/cm Grade Count:1
 0.600 - 0.700 J/cm
@Thickness 3.20 - 3.20 mm
1.12 - 1.31 ft-lb/in
@Thickness 0.126 - 0.126 in
Average value: 0.697 J/cm Grade Count:1
Izod Impact, Unnotched 3.20 - 5.34 J/cm6.00 - 10.0 ft-lb/inAverage value: 4.78 J/cm Grade Count:8
Izod Impact, Notched (ISO) 3.00 - 15.8 kJ/m²1.43 - 7.52 ft-lb/in²Average value: 7.27 kJ/m² Grade Count:3
 7.20 - 7.20 kJ/m²
@Temperature -30.0 - -30.0 °C
3.43 - 3.43 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 7.20 kJ/m² Grade Count:1
Izod Impact, Unnotched (ISO) 25.0 - 96.2 kJ/m²11.9 - 45.8 ft-lb/in²Average value: 48.7 kJ/m² Grade Count:3
 5.60 - 5.60 kJ/m²
@Temperature -30.0 - -30.0 °C
2.66 - 2.66 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 5.60 kJ/m² Grade Count:1
Charpy Impact Unnotched 2.50 - 9.73 J/cm²11.9 - 46.3 ft-lb/in²Average value: 4.42 J/cm² Grade Count:8
 0.640 - 5.00 J/cm²
@Temperature -30.0 - 0.000 °C
3.05 - 23.8 ft-lb/in²
@Temperature -22.0 - 32.0 °F
Average value: 3.13 J/cm² Grade Count:4
Charpy Impact, Notched 0.300 - 1.40 J/cm²1.43 - 6.66 ft-lb/in²Average value: 0.795 J/cm² Grade Count:19
 0.500 - 1.66 J/cm²
@Temperature -30.0 - 0.000 °C
2.38 - 7.90 ft-lb/in²
@Temperature -22.0 - 32.0 °F
Average value: 1.06 J/cm² Grade Count:5
Tensile Impact Strength 50.0 - 260 kJ/m²23.8 - 124 ft-lb/in²Average value: 190 kJ/m² Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+11 - 1.00e+17 ohm-cm1.00e+11 - 1.00e+17 ohm-cmAverage value: 2.23e+16 ohm-cm Grade Count:23
Surface Resistance 10000 - 6.00e+15 ohm10000 - 6.00e+15 ohmAverage value: 1.31e+15 ohm Grade Count:14
Dielectric Constant 2.00 - 3.402.00 - 3.40Average value: 2.91 Grade Count:13
Dielectric Strength 16.5 - 70.0 kV/mm420 - 1780 kV/inAverage value: 27.1 kV/mm Grade Count:14
Dissipation Factor 0.000800 - 0.01800.000800 - 0.0180Average value: 0.00335 Grade Count:12
Comparative Tracking Index 175 - 250 V175 - 250 VAverage value: 202 V Grade Count:13
 
Thermal PropertiesMetricEnglishComments
CTE, linear 30.0 - 50.0 µm/m-°C16.7 - 27.8 µin/in-°FAverage value: 38.3 µm/m-°C Grade Count:12
CTE, linear, Transverse to Flow 50.0 - 68.0 µm/m-°C27.8 - 37.8 µin/in-°FAverage value: 59.7 µm/m-°C Grade Count:9
Maximum Service Temperature, Air 115 - 160 °C239 - 320 °FAverage value: 148 °C Grade Count:9
Deflection Temperature at 0.46 MPa (66 psi) 127 - 254 °C260 - 489 °FAverage value: 157 °C Grade Count:20
Deflection Temperature at 1.8 MPa (264 psi) 105 - 232 °C221 - 450 °FAverage value: 138 °C Grade Count:42
Vicat Softening Point 130 - 230 °C266 - 446 °FAverage value: 162 °C Grade Count:16
Minimum Service Temperature, Air -40.0 °C-40.0 °FAverage value: -40.0 °C Grade Count:6
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:33
Oxygen Index 25.0 - 31.0 %25.0 - 31.0 %Average value: 28.5 % Grade Count:3
 
Processing PropertiesMetricEnglishComments
Processing Temperature 232 - 282 °C450 - 540 °FAverage value: 260 °C Grade Count:6
Nozzle Temperature 265 - 310 °C509 - 590 °FAverage value: 290 °C Grade Count:6
Melt Temperature 249 - 320 °C480 - 608 °FAverage value: 290 °C Grade Count:18
Mold Temperature 60.0 - 120 °C140 - 248 °FAverage value: 86.7 °C Grade Count:25
Drying Temperature 80.0 - 110 °C176 - 230 °FAverage value: 94.8 °C Grade Count:14
Moisture Content 0.0200 - 0.100 %0.0200 - 0.100 %Average value: 0.0500 % Grade Count:3
Injection Pressure 68.9 - 140 MPa10000 - 20300 psiAverage value: 99.6 MPa Grade Count:8
Vent Depth 0.00254 - 0.00381 cm0.00100 - 0.00150 inAverage value: 0.00339 cm Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for PPE/PPO + Carbon Fiber
EPICHEM Epiryl G2 PPO 20GF Polyphenylene oxide, 20% Glass Fiber
Overview of materials for Polyphenylene Ether, Molded
Overview of materials for Polyphenylene Ether, Impact Grade
Overview of materials for Polyphenylene Ether, 10% Glass Filled

O4412 / 78324

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.