MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

DuPont Mobility and Materials Zytel® (PA612) FG151 NC010 PA612  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 612 (PA612); Nylon 612, Unreinforced

Material Notes: Unreinforced Low Viscosity Polyamide 612 Developed for Food Contact Applications

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.06 g/cc0.0383 lb/in³DAM; ISO 1183
Water Absorption 3.0 %
@Thickness 2.00 mm
3.0 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Moisture Absorption 1.30 %
@Thickness 2.00 mm
1.30 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.013 cm/cm0.013 in/inDAM; ISO 294-4, 2577
 0.011 cm/cm
@Thickness 3.20 mm
0.011 in/in
@Thickness 0.126 in
DAM
Linear Mold Shrinkage, Transverse 0.014 cm/cm0.014 in/inDAM; ISO 294-4, 2577
 0.011 cm/cm
@Thickness 3.20 mm
0.011 in/in
@Thickness 0.126 in
DAM
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 114114DAM; ISO 2039-2
Tensile Strength, Yield 54.0 MPa7830 psi50%RH; ISO 527-1/-2
 62.0 MPa8990 psiDAM; ISO 527-1/-2
Elongation at Break 17 %17 %Nominal; DAM; ISO 527-1/-2
 >= 50 %>= 50 %Nominal; 50%RH; ISO 527-1/-2
Elongation at Yield 4.5 %4.5 %DAM; ISO 527-1/-2
 18 %18 %50%RH; ISO 527-1/-2
Tensile Modulus 1.70 GPa247 ksi50%RH; ISO 527-1/-2
 2.40 GPa348 ksiDAM; ISO 527-1/-2
Flexural Modulus 1.44 GPa209 ksi50%RH; ISO 178
 2.10 GPa305 ksiDAM; ISO 178
Poissons Ratio 0.380.38DAM
 0.420.4250%RH
Izod Impact, Notched (ISO)  3.00 kJ/m²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
50%RH; ISO 180/1A
 4.00 kJ/m²
@Temperature 23.0 °C
1.90 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 4.50 kJ/m²
@Temperature 23.0 °C
2.14 ft-lb/in²
@Temperature 73.4 °F
50%RH; ISO 180/1A
 4.50 kJ/m²
@Temperature -30.0 °C
2.14 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 180/1A
Charpy Impact Unnotched  4.00 J/cm²
@Temperature -30.0 °C
19.0 ft-lb/in²
@Temperature -22.0 °F
50%RH; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
50%RH; ISO 179/1eU
Charpy Impact, Notched  0.300 J/cm²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
50%RH; ISO 179/1eA
 0.350 J/cm²
@Temperature -30.0 °C
1.67 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 0.350 J/cm²
@Temperature 23.0 °C
1.67 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 179/1eA
 0.400 J/cm²
@Temperature 23.0 °C
1.90 ft-lb/in²
@Temperature 73.4 °F
50%RH; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.1 µin/in-°FDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 120 µm/m-°C66.7 µin/in-°FDAM; ISO 11359-1/-2
Specific Heat Capacity 2.75 J/g-°C0.657 BTU/lb-°FMelt
Thermal Conductivity 0.180 W/m-K1.25 BTU-in/hr-ft²-°FMelt
Melting Point 218 °C424 °F10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 135 °C275 °FDAM; ISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 62.0 °C144 °FDAM; ISO 75-1/-2
Vicat Softening Point 181 °C
@Load 5.10 kg
358 °F
@Load 11.2 lb
50°C/h; DAM; ISO 306
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 °C464 °FOptimum, Extrusion
 235 - 250 °C455 - 482 °FExtrusion
 250 °C482 °FOptimum, Injection
 230 - 290 °C446 - 554 °FInjection
Mold Temperature 50.0 - 90.0 °C122 - 194 °FInjection
Drying Temperature 75.0 °C167 °FExtrusion; Dehumidified Dryer
 75.0 - 80.0 °C
@Time 10800 - 14400 sec
167 - 176 °F
@Time 3.00 - 4.00 hour
Extrusion; Dehumidified Dryer
 80.0 °C
@Time 7200 - 14400 sec
176 °F
@Time 2.00 - 4.00 hour
Injection; Dehumidified Dryer
Moisture Content 0.060 - 0.15 %0.060 - 0.15 %
 
Descriptive Properties
FMVSS ClassBISO 3795 (FMVSS 302)
ISO designationISO 16396-PA612,,M1G1N,S12-020
Part Marking Code>PA612<ISO 11469
ProcessingInjection Molding
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationPA612ISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDSX5403m / 254520

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.