MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

AGC Fluon® P-63P PFA Resin
Categories: Polymer; Thermoplastic; Fluoropolymer; Perfluoroalkoxy (PFA)

Material Notes: Fluon® PFA (perfluoroalkoxy) is a melt-processible copolymer of tetrafluoroethylene and a perfluorinated vinyl ether. Fluon® PFA has chemical, electrical, and thermal properties almost identical to its close chemical cousin, polytetrafluoroethylene (PTFE), yet can be processed by conventional extrusion, injection molding, blow molding, and transfer molding techniques. This material can be used over a wide range of temperatures (-200°C to 260°C). It is available as a 1/8” pellet.

Benefits:

  • High Resistance to Heat
  • Excellent Chemical Resistance
  • Low Smoke and Flame Characteristics. Fluon® PFA is rated 94V-0 by Underwriters Laboratories Inc.
  • Outstanding Resistance to Weather and Aging
  • Excellent Dielectric Properties
  • Non-Stick Characteristics
Applications:
  • Tubing and Pipe
  • Film and Sheets
  • Valves, Fittings, and Housings
  • Wire and Cable

Information provided by AGC Chemicals Americas Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.14 g/cc2.14 g/ccASTM D792
Water Absorption <= 0.030 %
@Time 86400 sec
<= 0.030 %
@Time 24.0 hour
ASTM D570
Melt Flow 12 g/10 min12 g/10 minASTM D3159
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6060ASTM D2240
Tensile Strength  8.96 MPa
@Temperature 250 °C
1300 psi
@Temperature 482 °F
ASTM D638
 32.0 MPa
@Temperature 23.0 °C
4640 psi
@Temperature 73.4 °F
ASTM D638
 50.0 MPa
@Temperature -79.0 °C
7250 psi
@Temperature -110 °F
 110 MPa
@Temperature -129 °C
16000 psi
@Temperature -200 °F
 140 MPa
@Temperature -198 °C
20300 psi
@Temperature -324 °F
Elongation at Break  1.0 %
@Temperature -198 °C
1.0 %
@Temperature -324 °F
 1.0 %
@Temperature -129 °C
1.0 %
@Temperature -200 °F
 9.0 %
@Temperature -79.0 °C
9.0 %
@Temperature -110 °F
 410 %
@Temperature 23.0 °C
410 %
@Temperature 73.4 °F
ASTM D638
 600 %
@Temperature 250 °C
600 %
@Temperature 482 °F
ASTM D638
Flexural Strength  2.50 MPa
@Temperature 250 °C
363 psi
@Temperature 482 °F
ASTM D790
 8.00 MPa
@Temperature 100 °C
1160 psi
@Temperature 212 °F
ASTM D790
 19.0 MPa
@Temperature 25.0 °C
2760 psi
@Temperature 77.0 °F
ASTM D790
Flexural Modulus  0.0200 GPa
@Temperature 250 °C
2.90 ksi
@Temperature 482 °F
ASTM D790
 0.180 GPa
@Temperature 100 °C
26.1 ksi
@Temperature 212 °F
ASTM D790
 0.630 GPa
@Temperature 25.0 °C
91.4 ksi
@Temperature 77.0 °F
ASTM D790
 1.60 GPa
@Temperature -79.0 °C
232 ksi
@Temperature -110 °F
 4.00 GPa
@Temperature -129 °C
580 ksi
@Temperature -200 °F
Flex Crack Resistance 2500025000Cycles per MIT Folding Endurance; ASTM D2176
Izod Impact, Notched  6.80 J/cm
@Temperature -40.0 °C
12.7 ft-lb/in
@Temperature -40.0 °F
ASTM D256
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ASTM C256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+18 ohm-cm>= 1.00e+18 ohm-cmASTM D257
Dielectric Constant 2.07
@Frequency 1e+6 Hz
2.07
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 74.8 kV/mm1900 kV/inASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear  >= 90.0 µm/m-°C
@Temperature -100 - -75.0 °C
>= 50.0 µin/in-°F
@Temperature -148 - -103 °F
ASTM D696
 >= 110 µm/m-°C
@Temperature -75.0 - -15.0 °C
>= 61.1 µin/in-°F
@Temperature -103 - 5.00 °F
ASTM D696
 130 µm/m-°C
@Temperature 0.000 - 100 °C
72.0 µin/in-°F
@Temperature 32.0 - 212 °F
ASTM D696
 >= 140 µm/m-°C
@Temperature -15.0 - 100 °C
>= 77.8 µin/in-°F
@Temperature 5.00 - 212 °F
ASTM D696
 >= 160 µm/m-°C
@Temperature 100 - 150 °C
>= 88.9 µin/in-°F
@Temperature 212 - 302 °F
ASTM D696
 >= 210 µm/m-°C
@Temperature 150 - 210 °C
>= 117 µin/in-°F
@Temperature 302 - 410 °F
ASTM D696
Specific Heat Capacity 1.05 J/g-°C0.251 BTU/lb-°F
Melting Point 310 °C590 °FASTM D3459
Maximum Service Temperature, Air 260 °C500 °F
Deflection Temperature at 0.46 MPa (66 psi) 92.0 °C198 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 57.0 °C135 °FASTM D648
Vicat Softening Point 281 °C538 °F50°C/h; JIS K7206
Flammability, UL94 V-0V-0
Oxygen Index >= 95 %>= 95 %ASTM D2863
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.351.35ASTM D542
 
Descriptive Properties
Heat of Combustion2200 BTU/lbASTM D240

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AGC Fluon® P-66P PFA Resin
AGC Fluon® P-65P PFA Resins
AGC Fluon® P-62XP PFA Resin
AGC Fluon® C88AXMP-HT ETFE
AGC Fluon® C-88AXMP ETFE

PAGCX259 / 191368

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.