MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

KEP Kepital® FG2025 Acetal Copolymer, 25% Glass Fiber
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, 30% Glass Fiber Reinforced

Material Notes: 25% glass fiber filled medium viscosity grade good for general injection molding. FG2025 is good for parts requiring very high stiffness, strength, creep resistance, and HDT.

Information provided by KEP Americas.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.59 g/cc0.0574 lb/in³ISO 1183
Water Absorption 0.20 %0.20 %ISO 62
Linear Mold Shrinkage, Flow 0.0050 cm/cm0.0050 in/int = 3 mm
Melt Flow 7.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
7.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 160 MPa23200 psi50 mm/min; ISO 527
Elongation at Break 3.0 %3.0 %50 mm/min; ISO 527
Flexural Strength 220 MPa31900 psiISO 178
Flexural Modulus 8.25 GPa1200 ksiISO 178
Charpy Impact, Notched 0.850 J/cm²4.04 ft-lb/in²ISO 179
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cmIEC 60093
Surface Resistance 1.00e+16 ohm1.00e+16 ohmIEC 60093
Dielectric Strength 23.0 kV/mm584 kV/inIEC 60243
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.0 - 30.0 µm/m-°C11.1 - 16.7 µin/in-°FISO 11359
Melting Point 165 °C329 °FISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 162 °C324 °FISO 75

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
KEP Kepital® FG1025 Acetal Copolymer, 25% Glass Fiber
Celanese Celcon® GC25T POM, 25% Glass Reinforced
Overview of materials for Acetal Copolymer, Unreinforced
KEP Kepital® FG2025 25% Glass Fiber Reinforced Acetal Copolymer
Celanese Celstran® POM-GF25-04 AF3001 POM, 25% Glass Reinforced

PKEP9903 / 185579

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.