MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Mocom (ALBIS) ALCOM® PA66 910/1 AR20 Nylon 66, 20% Aramid Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Aramid Fiber Filled

Material Notes: Base Polymer: Polyamide 66

Filler/Additive System: 20% aramid

Special Features: Improved sliding/wear, heat ageing stabilization, high stiffness

Market Segment: Automotive, Machinery

Typical Applications: Functional components

Information provided by Albis Plastics

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.18 g/cc0.0426 lb/in³ISO 1183
Storage Temperature <= 30.0 °C<= 86.0 °Fdry, protected from light
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 72.0 MPa10400 psiISO 527
Elongation at Break 2.7 %2.7 %ISO 527
Tensile Modulus 3.70 GPa537 ksiISO 527
Flexural Strength 115 MPa16700 psiISO 178
Flexural Modulus 3.55 GPa515 ksiISO 178
Charpy Impact Unnotched 1.60 J/cm²7.61 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 0.200 J/cm²0.952 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 100 °C212 °FISO 75-1/-2
Vicat Softening Point 247 °C477 °FB50; ISO 306
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 - 300 °C536 - 572 °FInjection molding
Mold Temperature 80.0 - 120 °C176 - 248 °FInjection molding
Drying Temperature <= 80.0 °C
@Time 7200 - 43200 sec
<= 176 °F
@Time 2.00 - 12.0 hour
in a dry air (desiccant) dryer
 
Descriptive Properties
Base PolymerPolyamide 66

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Asahi Kasei Leona™ 14025 Polyamide 66, Heat Stabilized
Asahi Kasei Leona™ 13G50 Polyamide 66, GF Reinforced
Asahi Kasei Leona™ 13005 Polyamide 66, General Purpose
Arkema Orgalloy® RS 6630 BLACK Polyamide 6.6 Alloy 30% Glass Fiber reinforced
Arkema Orgalloy® RS 6620 NAT Polyamide 6.6 Alloy 20% Glass Fiber reinforced

PALBIS8091 / 242150

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.