Asahi Kasei Leona™ CR103 Polyamide 66, MF reinforced and Heat Stabilized
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
Material Notes:
Applications: Automotive parts, electrical & electronic parts, parts for office furnishings.
Information provided by Asahi Kasei Corp.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.45
g/cc
1.45
g/cc
Dry as Molded; ASTM D792
Density
1.45
g/cc
0.0524
lb/in³
Dry as Molded; ISO 1183
Moisture Absorption at Equilibrium
1.0 %
@Temperature 23.0 °C
1.0 %
@Temperature 73.4 °F
50% RH
1.5 %
@Temperature 23.0 °C
1.5 %
@Temperature 73.4 °F
50% RH; ISO 62
Linear Mold Shrinkage, Flow
0.0050
-
0.011
cm/cm
0.0050
-
0.011
in/in
Asahi Kasei
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell M
74
74
Conditioned at 50% RH; ISO 2039
94
94
Dry as Molded; ISO 2039
Hardness, Rockwell R
94
94
Conditioned at 50% RH; ISO 2039
120
120
Dry as Molded; ISO 2039
Tensile Strength at Break
100
MPa
14500
psi
Conditioned at 50% RH; ISO 527
131
MPa
19000
psi
Dry as Molded; ISO 527
Tensile Strength
106
MPa
15400
psi
Conditioned at 50% RH; ASTM D638
139
MPa
20200
psi
Dry as Molded; ASTM D638
Elongation at Break
4.0 %
4.0 %
Dry as Molded; ISO 527
7.0 %
7.0 %
Conditioned at 50% RH; ISO 527
Tensile Modulus
5.20
GPa
754
ksi
Conditioned at 50% RH; ISO 527
8.10
GPa
1170
ksi
Dry as Molded; ISO 527
Flexural Strength
143
MPa
20700
psi
Conditioned at 50% RH; ISO 178
203
MPa
29400
psi
Dry as Molded; ISO 178
Flexural Modulus
4.20
GPa
609
ksi
Conditioned at 50% RH; ISO 178
6.70
GPa
972
ksi
Dry as Molded; ISO 178
Izod Impact, Notched
0.510
J/cm
0.955
ft-lb/in
Dry as Molded; ASTM D256
0.590
J/cm
1.11
ft-lb/in
Conditioned at 50% RH; ASTM D256
Charpy Impact, Notched
0.460
J/cm²
2.19
ft-lb/in²
Dry as Molded; ISO 179
0.550
J/cm²
2.62
ft-lb/in²
Conditioned at 50% RH; ISO 179
Thermal Properties
Metric
English
Comments
CTE, linear
40.0
µm/m-°C
22.2
µin/in-°F
Dry as Molded; ASTMD 696
Deflection Temperature at 0.46 MPa (66 psi)
250
°C
482
°F
Dry as Molded; ISO 75
Deflection Temperature at 1.8 MPa (264 psi)
240
°C
464
°F
Dry as Molded; ISO 75
Flammability, UL94
HB
@Thickness 0.750 mm
HB
@Thickness 0.0295 in
Dry as Molded
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PASAHI8156 / 221183
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.